Light leveling dry-mixed mortar
A technology of leveling dry powder and mortar, which is applied in the field of lightweight leveling dry powder mortar, which can solve the problems of low construction efficiency, unfavorable health of on-site construction personnel, and influence on the service life of buildings, so as to reduce construction labor intensity and achieve good leveling performance in thick layers. Conducive to the effect of resource utilization
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0042] Desulfurized gypsum 60%
[0043] Fly Ash 10%
[0044] Ground calcium carbonate 20%
[0045] Cement 5%
[0046] Sand 2%
[0047] Lightweight aggregate 1%
[0049] Magnesium Aluminum Silicate 0.5%
[0050] Redispersible latex powder 0.3%
[0051] Cellulose ether 0.2%
[0052] Retarder 0.1%
[0053] Water reducer 0.8%;
[0054] Redispersible latex powder is vinyl acetate;
[0055] The viscosity of cellulose ether is 70000cps;
[0056] The retarder is citric acid.
[0057] Mix and stir for 10 minutes according to the ratio of light leveling dry powder mortar and water 2:1 (weight ratio), spread it on the wall and ceiling, and then scrape and compact it.
[0058] In this example, the lightweight leveling mortar has good cohesiveness and high resistance to deformation. According to the test method of "Test Methods for Physical Properties of Dry-Mixed Mortar" GB / T 29756-2013, the compressive strength is greater than 4.1Mpa. The bonding...
Embodiment 2
[0061] Desulfurization gypsum 70%
[0062] Fly Ash 2%
[0063] Ground calcium carbonate 20%
[0064] Cement 2%
[0065] Sand 2%
[0066] Lightweight aggregate 1%
[0067] Starch ether 0.1%
[0068] Magnesium Aluminum Silicate 0.5%
[0069] Redispersible latex powder 1%
[0070] Cellulose ether 0.5%
[0071] Retarder 0.15%
[0072] Water reducer 0.75%;
[0073] Redispersible latex powder is acrylate;
[0074] The viscosity of cellulose ether is 150000cps;
[0075] The retarder is tartaric acid.
[0076] Mix and stir for 15 minutes according to the ratio of light leveling dry powder mortar and water 1.5:1 (weight ratio), spread it on the wall and ceiling, and then scrape and compact it.
[0077] In this example, the lightweight leveling mortar has good cohesiveness and high resistance to deformation. According to the test method of "Test Method for Physical Properties of Dry-Mixed Mortar" GB / T 29756-2013, the compressive strength is greater than 4.3Mpa. The bondin...
Embodiment 3
[0080] Desulfurized gypsum 65%
[0081] Fly Ash 5%
[0082] Ground calcium carbonate 20%
[0083] Cement 2%
[0084] Sand 2%
[0085] Lightweight aggregate 1%
[0086] Starch ether 0.1%
[0087] Magnesium Aluminum Silicate 0.5%
[0088] Redispersible latex powder 1%
[0089] Cellulose ether 0.5%
[0090] Retarder 0.1%
[0091] Water reducer 0.8%
[0092] Gray cement PO52.5 2%;
[0093] The redispersible latex powder is a 1:1 mixture of vinyl acetate and acrylate by weight;
[0094] The viscosity of cellulose ether is 120000cps;
[0095] The retarder is sodium citrate.
[0096] The lightweight aggregates are fly ash floating beads, vitrified beads, expanded perlite, polystyrene particles, etc.
[0097] Mix and stir for 15 minutes according to the ratio of light leveling dry powder mortar and water 1.5:1 (weight ratio), spread it on the wall and ceiling, and then scrape and compact it.
[0098] In this example, the lightweight leveling mortar has good cohesiveness ...
PUM
Property | Measurement | Unit |
---|---|---|
Viscosity | aaaaa | aaaaa |
Compressive strength | aaaaa | aaaaa |
Bond strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com