Multi-ion antibacterial material
An antibacterial material and multi-ion technology, applied in the field of antibacterial materials, can solve the problems of low antibacterial properties and low service life of antibacterial materials, and achieve the effects of avoiding low antibacterial properties, long service life, and enhancing ionization activity and strength.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0040] A multi-ion antibacterial material is prepared by the following method:
[0041] (1) First mix silicon dioxide with water at a mass ratio of 0.55:1, then add it to 0.5 times the mass of water, and stir to obtain a suspension; mix silver nitrate, zinc nitrate and magnesium oxide with the suspension in mass ratio 1. Mix 8:1 to obtain three solutions; heat the three solutions with water bath to 30°C, then mix the three solutions and keep stirring until completely dissolved to obtain solution A.
[0042] (2) Melt copper first, then add zinc to melt and mix zinc and copper, and then add charcoal powder, wherein the mass ratio of copper, zinc, and charcoal powder is 1:1.5:3; after mixing evenly, cool down and grind to obtain composite yellow copper powder.
[0043] (3) Add composite brass powder into solution A according to the mass ratio of 1.2:2 to form mixture B; a nitric acid solution with a pH value of 4.6, add mixture B to a nitric acid solution twice its mass; heat up...
Embodiment 2
[0045] A multi-ion antibacterial material is prepared by the following method:
[0046] (1) First mix silicon dioxide with water at a mass ratio of 0.5:1, then add it to 0.4 times the mass of water, and stir to obtain a suspension; mix silver nitrate, zinc nitrate and magnesium oxide with the suspension in mass ratio 1. 5:1 mixing to obtain three solutions; the three solutions were heated to 28°C in a water bath, and then the three solutions were mixed and continuously stirred until completely dissolved to obtain solution A.
[0047] (2) Melt copper first, then add zinc to melt and mix zinc and copper, and then add charcoal powder, wherein the mass ratio of copper, zinc, and charcoal powder is 1:1.4:2.8; after mixing evenly, cool down and grind to obtain composite yellow copper powder.
[0048] (3) Join composite brass powder in solution A by mass ratio 1.2:2, form mixture B; Prepare the nitric acid solution that pH value is 4.2, join mixture B in the nitric acid solution of ...
Embodiment 3
[0050] A multi-ion antibacterial material is prepared by the following method:
[0051] (1) First mix silicon dioxide with water at a mass ratio of 0.6:1, then add it to 0.6 times the mass of water, and stir to obtain a suspension; mix silver nitrate, zinc nitrate and magnesium oxide with the suspension by mass ratio 2:1 mixing to obtain three solutions; the three solutions were heated to 35°C in a water bath, and then the three solutions were mixed and continuously stirred until completely dissolved to obtain solution A.
[0052] (2) Melt copper first, then add zinc to melt and mix zinc and copper, and then add charcoal powder, wherein the mass ratio of copper, zinc, and charcoal powder is 1:1.6:3.2; after mixing evenly, cool down and grind to obtain composite yellow copper powder.
[0053] (3) Join composite brass powder in solution A by mass ratio 1.1-1.3:2, form mixture B; Prepare the nitric acid solution that pH value is 5, join mixture B in the nitric acid solution of i...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology