A kind of antirust agent, water-soluble technology, applied in the field of water-soluble antirust agent and its preparation, can solve the problems of dust affecting antirust performance, strong toxicity of antirust agent, polluting the environment, etc., and achieve excellent antirust performance and corrosion resistance Good performance, good anti-corrosion effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] A water-soluble antirust agent prepared from the following ingredients in parts by weight: 2 parts of hydroxyl silicone oil emulsion, 1 part of sodium silicate, 5 parts of phytic acid, 0.2 part of gluconic acid, 0.1 part of calcium hydrogen phosphite, poly 2 parts of aspartic acid, 0.2 part of phenylalanine, 0.5 part of sodium tetraborate, 1 part of sulfonated lignin, 0.5 part of polyvinyl alcohol, 0.2 part of diethylenetriamine, 0.5 part of sodium citrate, and 80 parts of distilled water.
[0017] The preparation method of above-mentioned water-soluble antirust agent is:
[0018] The first step: mix phytic acid, gluconic acid, calcium hydrogen phosphite, polyaspartic acid, phenylalanine, sodium tetraborate, sulfonated lignin, sodium citrate and distilled water at a speed of 200r / min Stir for 20 minutes;
[0019] Step 2: Add hydroxy silicone oil emulsion, heat to 75°C and stir for 10 minutes;
[0020] Step 3: Lower the temperature to 50°C, add sodium silicate, polyvin...
Embodiment 2
[0023] A water-soluble antirust agent, prepared from the following ingredients in parts by weight: 3 parts of hydroxyl silicone oil emulsion, 1.5 parts of sodium silicate, 5.2 parts of phytic acid, 0.3 parts of gluconic acid, 0.15 parts of calcium hydrogen phosphite, poly 2.5 parts of aspartic acid, 0.3 parts of phenylalanine, 0.6 parts of sodium tetraborate, 1.2 parts of sulfonated lignin, 0.6 parts of polyvinyl alcohol, 0.3 parts of diethylenetriamine, 0.6 parts of sodium citrate, and 85 parts of distilled water.
[0024] The preparation method of above-mentioned water-soluble antirust agent is:
[0025] The first step: mix phytic acid, gluconic acid, calcium hydrogen phosphite, polyaspartic acid, phenylalanine, sodium tetraborate, sulfonated lignin, sodium citrate and distilled water at a speed of 250r / min Stir for 25 minutes;
[0026] Step 2: Add hydroxy silicone oil emulsion, heat to 76°C and stir for 15 minutes;
[0027] Step 3: Lower the temperature to 55°C, add sodiu...
Embodiment 3
[0030] A water-soluble antirust agent, prepared from the following ingredients in parts by weight: 3.5 parts of hydroxyl silicone oil emulsion, 2 parts of sodium silicate, 5.5 parts of phytic acid, 0.35 parts of gluconic acid, 0.2 parts of calcium hydrogen phosphite, poly 3 parts of aspartic acid, 0.35 parts of phenylalanine, 0.75 parts of sodium tetraborate, 1.5 parts of sulfonated lignin, 0.65 parts of polyvinyl alcohol, 0.35 parts of diethylenetriamine, 0.75 parts of sodium citrate, and 90 parts of distilled water.
[0031] The preparation method of above-mentioned water-soluble antirust agent is:
[0032] The first step: mix phytic acid, gluconic acid, calcium hydrogen phosphite, polyaspartic acid, phenylalanine, sodium tetraborate, sulfonated lignin, sodium citrate and distilled water at a speed of 300r / min Stir for 25 minutes;
[0033] Step 2: Add hydroxy silicone oil emulsion, heat to 77°C and stir for 20 minutes;
[0034] Step 3: Lower the temperature to 55°C, add so...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com