Embodiment 1~9
[0057] A. Add the components 1 to 9 in Table 1-1 and 1-2 into the production tank, turn on the high-speed disperser equipment, and adjust the dispersion speed to 350r / min; add the example numbers in Table 1 in turn For components ②~⑧ of 1~9, adjust the dispersion speed to 400r / min, and disperse and stir for 5min;
[0058] B. Adjust the dispersion speed to 800r / min~1200r / min (adjust according to the production volume), and add the ⑨~ of the embodiment numbers 1~9 in Table 1-1 and 1-2 in turn. Components, disperse and stir for 30 minutes, and enter the next process stage after the fineness is less than or equal to 35 μm;
[0059] C. Adjust the dispersing speed to 500r / min, and add the ingredients of Example Nos. 1 to 9 in Tables 1-1 and 1-2 in turn. Components, dispersed for 5 minutes;
[0060] D. Adjust the dispersing speed to 400r / min, and add the ingredients of Example Nos. 1 to 9 in Tables 1-1 and 1-2 in turn. Components, dispersed for 5 minutes;
[0061] E. Adjust th...
Embodiment 10
[0063] The stain-resistant white latex paint provided by the present embodiment, its raw material components include:
[0064] 20% water, 4% water-based wax, 30% silicone acrylic polymer emulsion, 10% additives, 21% pigments, and 15% fillers.
[0065] Its preparation method is as follows:
[0066] A. Add water 150kg, slow-release formaldehyde preservative 3kg, hydroxyethyl ether cellulose 4kg, soybean lecithin 2.5kg, sodium hexametaphosphate 10kg, silicone oil defoamer 4kg, ethylene glycol 30kg, AMP-952kg, Disperse and stir evenly;
[0067] B. Add 50kg of water, 210kg of zinc oxide and 150kg of 1250 mesh talcum powder in sequence, and enter the next step after the fineness is ≤35μm;
[0068] C. Add 40kg of water-based wax and 26kg of Texanol in turn, disperse and stir evenly;
[0069] D. Add 300kg of silicone acrylic polymer emulsion, AMP-951kg and 4.5kg of liquid metal soap emulsion in turn, disperse and stir evenly;
[0070] E. Add 10kg of aluminum stearate and 3kg of ac...
Embodiment 11
[0072] The stain-resistant white latex paint provided by the present embodiment, its raw material components include:
[0073] 40% water, 1% water-based wax, 5% silicone acrylic polymer emulsion, 25% second emulsion, 5% additives, 19% pigment, and 5% filler.
[0074] Its preparation method is as follows:
[0075] A. First add 250kg of water to the production tank, turn on the high-speed disperser equipment, and adjust the dispersing speed to 350r / min. Add 1 kg of Casson and Bropol composite preservative, 1 kg of methyl cellulose, 0.5 kg of pull-off powder BX, 3 kg of ammonium salt, 4 kg of polyether defoamer, 20 kg of propylene glycol, and 0.5 kg of AMP-95, and adjust the dispersion speed. To 400r / min, disperse and stir for 5min to enter the next process stage;
[0076] B. Adjust the dispersion speed to 800r / min-1200r / min (adjusted according to the production volume), add 150kg of water, 190kg of barium sulfate, and 50kg of 1250 mesh calcined kaolin in turn, disperse and sti...
PUM
Property | Measurement | Unit |
---|---|---|
particle size (mesh) | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com