A manufacturing method and technology of oriented silicon, applied in the field of electrical steel manufacturing, can solve the problems of many product defects, easy cracking of thin strips, high energy consumption, etc., and achieve the effect of simplifying the production process, simple manufacturing method and low energy consumption
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0039] The molten steel composition of ultra-thin grain-oriented silicon steel sheet is C 0.04%, Si 3.0%, Mn 0.18%, S 0.022%, Als 0.025%, N 0.0095%, O8 1.80T, iron loss P 10 / 400 6.6W / kg, P 10 / 1000 22.0 W / kg, thickness 0.1mm;
[0040] The molten steel for smelting has the same composition as above;
[0041] A twin-roll strip continuous casting device is used to pour molten steel through the tundish into a cavity composed of two crystallization rollers and two side sealing plates to form a molten pool. The upper surface superheat of the molten pool is controlled at 40°C, and the molten steel in the molten pool Solidified with the rotation of the crystal roll and exported at a speed of 40m / min to obtain a cast belt;
[0042] The cast strip is cooled by the cooling unit at a speed of 60°C / s and then hot-rolled. The rolling start temperature is 1000°C, the hot-rolling reduction rate is 33.3%, the final rolling temperature is above 800°C, and the hot-rolling temperature is 60°C / s....
Embodiment 2
[0050] The molten steel composition of ultra-thin grain-oriented silicon steel sheet is C 0.002%, Si 2.8%, Mn 0.05%, S 0.015%, Als 0.005%, N 0.003%, Cu 0.3%, Sn 0.1%, O8 1.72T, iron loss P 10 / 400 is 8.1W / kg, P 10 / 1000 19.2W / kg, thickness 0.05mm;
[0051] Manufacturing method is the same as embodiment 1, and difference is:
[0052] (1) Molten steel for smelting, with the same composition as above;
[0053] (2) The superheat degree on the upper surface of the molten pool is 10°C, and the molten steel is exported at a speed of 60m / min;
[0054] (3) The cast strip is cooled at a rate of 20 °C / s, the hot rolling start temperature is 900 °C, the reduction rate is 15%, and the hot rolling is cooled at a rate of 20 °C / s;
[0055] (4) The normalization treatment temperature is 850°C, the time is 10min, and the normalization treatment cooling rate is 5°C / s;
[0056] (5) The first cold rolling reduction rate is 40%; the intermediate annealing temperature is 800°C, and the time is 10 ...
Embodiment 3
[0061] The molten steel composition of ultra-thin grain-oriented silicon steel sheet is C 0.08%, Si 3.4%, Mn 0.30%, S 0.04%, Als 0.05%, N 0.007%, Cu 0.6%, Sn 0.2%, O8 1.83T, iron loss P 10 / 400 is 7.1 W / kg, P 10 / 1000 27.2W / kg, thickness 0.15mm;
[0062] Manufacturing method is the same as embodiment 1, and difference is:
[0063] (1) Molten steel for smelting, with the same composition as above;
[0064] (2) The superheat degree on the upper surface of the molten pool is 70°C, and the molten steel is exported at a speed of 20m / min;
[0065] (3) The cast strip is cooled at a rate of 100 °C / s, the hot rolling start temperature is 1150 °C, the reduction rate is 50%, and the hot rolling is cooled at a rate of 100 °C / s;
[0066] (4) The normalization treatment temperature is 1150°C, the time is 1min, and the normalization treatment cooling rate is 50°C / s;
[0067] (5) The first cold rolling reduction rate is 70%; the intermediate annealing temperature is 1100 ° C, and the time i...
PUM
Property | Measurement | Unit |
---|---|---|
thickness | aaaaa | aaaaa |
width | aaaaa | aaaaa |
height | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com