A kind of high-silicon iron tailings foam glass-ceramics and its production method
A technology of foamed glass-ceramic and high-silicon iron tailings is applied in the field of building and engineering thermal insulation and thermal insulation materials, which can solve the problems of high cost, high compressive strength and low thermal conductivity of foamed glass-ceramic, and solve pollution problems. Hazard problem, good performance, low production cost effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0037] Embodiment one: the method for producing foamed glass-ceramic by utilizing high-silicon tailings, comprises the following steps:
[0038] (1) Raw materials: Weigh 90wt% of high-silicon iron tailings, 1wt% of foaming agent, and 9wt% of additives; Talc is mixed at a mass ratio of 5:0.5;
[0039] (2) Put each raw material in a ball mill, and ball mill until the particle size of the mixture is 200 mesh;
[0040] (3) Spread the mixture into the mold for molding;
[0041] (4) Push the formed mixture into the tunnel kiln, and go through preheating, sintering, foaming, quenching, crystallization, and annealing processes to obtain a foamed glass-ceramic blank. The specific requirements are as follows:
[0042] 1) Preheating: Gradually raise the temperature of the formed mixture from room temperature to 600°C at a heating rate of 2°C / min, and keep it at this temperature for 30 minutes;
[0043] 2) Sintering: Gradually raise the temperature from 600°C to 1000°C at a heating rat...
Embodiment 2
[0049] Embodiment 2 The method for producing foamed glass-ceramics by using high-silicon tailings comprises the following steps:
[0050] (1) Raw materials: Weigh 80wt% of high-silicon iron tailings, 1wt% of foaming agent, and 19wt% of additives; Stone and talc are mixed at a mass ratio of 5:0.5;
[0051] (2) Put each raw material in a ball mill, and ball mill until the particle size of the mixture is 300 mesh;
[0052] (3) Put the mixture into the mold and press it into shape;
[0053](4) The formed mixture is pushed into the tunnel kiln, and after preheating, sintering, foaming, quenching, crystallization, and annealing processes, the foamed glass-ceramic blank is obtained. The specific requirements are as follows:
[0054] 1) Preheating: Gradually raise the temperature of the formed mixture from room temperature to 600°C at a heating rate of 5°C / min, and keep it at this temperature for 30 minutes;
[0055] 2) Sintering: Gradually raise the temperature from 600°C to 1000°...
Embodiment 3
[0061] Embodiment 3 The method for producing foamed glass-ceramics by utilizing high-silicon tailings comprises the following steps:
[0062] (1) Weigh 70wt% of raw material high-silicon iron tailings, 1wt% of foaming agent, and 29wt% of additives; Mixed with a mass ratio of 5:0.5;
[0063] (2) Put each raw material in a ball mill, and ball mill until the particle size of the mixture is 250 mesh;
[0064] (3) Put the mixture into the mold and press it into shape;
[0065] (4) Push the formed mixture into a tunnel kiln, and undergo preheating, sintering, foaming, quenching, crystallization, and annealing processes to obtain rough foamed glass-ceramics. The specific requirements are as follows:
[0066] 1) Preheating: Gradually raise the temperature of the molded mixture from room temperature to 600°C at a heating rate of 5°C / min, and keep it at this temperature for 30 minutes;
[0067] 2) Sintering: Gradually raise the temperature from 600°C to 1000°C at a heating rate of 5°...
PUM
Property | Measurement | Unit |
---|---|---|
compressive strength | aaaaa | aaaaa |
water absorption | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com