A production method and technology for handicrafts, applied in the direction of manufacturing tools, wood processing utensils, botanical equipment and methods, etc., can solve the problems of destroying the ornamental and collection value of handicrafts, occurrence of moth-eaten or other corrosion phenomena, etc., to achieve strong adhesion, Good wettability and stability, good anti-mold effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] The making method of wooden handicraft is carried out as follows:
[0025] (1) Peeling: Use a wood peeling machine to peel off the outer skin of the original wood;
[0026] (2) Anti-corrosion: soak the peeled wood in anti-corrosion solution for anti-corrosion treatment; the steps of anti-corrosion treatment are:
[0027] a. Put the wood in a closed pressure impregnation tank, and add preservatives composed of the following components by weight percentage to fill the tank: 3% disodium octaborate tetrahydrate, 1% copper citrate, 4% ammonium bisulfate, Ammonium molybdate 3%, boric acid 4%, polyvinyl alcohol 3%, p-chloro-m-xylenol 2%, tetrakis hydroxymethyl phosphorus sulfate 4%, sorbitan monostearate 3%, dodecylbenzene Sodium sulfonate 4%, the balance is water;
[0028] b. Pressurize to 1Mpa and keep it for about 5 hours;
[0029] c. Release the pressure and empty the preservative;
[0030] d. Remove the wood from the tank.
[0031] (3) Drying: Seal the wood in a stea...
Embodiment 2
[0038] The making method of wooden handicraft is carried out as follows:
[0039] (1) Peeling: Use a wood peeling machine to peel off the outer skin of the original wood;
[0040] (2) Anti-corrosion: soak the peeled wood in anti-corrosion solution for anti-corrosion treatment; the steps of anti-corrosion treatment are:
[0041] a. Put the wood in a closed pressure impregnation tank, and add preservatives composed of the following components by weight percentage to fill the tank: 2% disodium octaborate tetrahydrate, 1% copper citrate, 5% ammonium bisulfate, Ammonium molybdate 5%, boric acid 2%, polyvinyl alcohol 1%, p-chloro-m-xylenol 3%, tetrakis hydroxymethyl phosphorus sulfate 3%, sorbitan monostearate 2%, dodecylbenzene Sodium sulfonate 1%, the balance is water;
[0042] b. Pressurize to 0.8Mpa and keep it for about 4 hours;
[0043] c. Release the pressure and empty the preservative;
[0044] d. Remove the wood from the tank.
[0045] (3) Drying: Seal the wood in a st...
Embodiment 3
[0052] The making method of wooden handicraft is carried out as follows:
[0053] (1) Peeling: Use a wood peeling machine to peel off the outer skin of the original wood;
[0054] (2) Anti-corrosion: soak the peeled wood in anti-corrosion solution for anti-corrosion treatment; the steps of anti-corrosion treatment are:
[0055] a. Put the wood in a closed pressure impregnation tank, and add preservatives consisting of the following components in weight percentages to the full tank: 2% disodium octaborate tetrahydrate, 2% copper citrate, 4% ammonium bisulfate, Ammonium molybdate 6%, boric acid 3%, polyvinyl alcohol 2%, p-chloro-m-xylenol 2%, tetrakis hydroxymethyl phosphorus sulfate 3%, sorbitan monostearate 3%, dodecylbenzene Sodium sulfonate 3%, the balance is water;
[0056] b. Pressurize to 0.9Mpa and keep it for about 3 hours;
[0057] c. Release the pressure and empty the preservative;
[0058] d. Remove the wood from the tank.
[0059] (3) Drying: Seal the wood in a...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com