A porous partition wall and lightweight technology, applied in the field of building materials, can solve the problems of low thermal conductivity, sound insulation effect, uneven hole formation, poor heat insulation effect, etc., achieve good fire prevention effect, low production energy consumption, and strong durability Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0023] Recipe 1:
[0024] Component Formula (wt%) 100 mesh coal gangue15 600 mesh slag30 First grade fly ash21.5 Water glass (m=1.5)25 Calcium stearate0.5 Aluminum powder foaming agent1 water7 total100
[0025] The preparation method is as follows:
[0026] (1) Prepare various raw materials in proportion;
[0027] (2) The coal gangue, slag, fly ash, and calcium stearate are mixed and stirred evenly into powder material according to the proportion;
[0028] (3) Add modulus m=1.5 water glass and water to the mixed powder material and stir evenly to obtain slurry;
[0029] (4) Add the aluminum powder foaming agent to the slurry, mix and stir evenly, then pour it into the mold and foam it into a green body;
[0030] (5) Cut the cast body after 8 hours of static stop at room temperature.
[0031] (6) Put the cut plate into an autoclave for autoclave, the pressure is 10×Pa, the temperature is 205℃, and the autoclave time is 6h.
[0032] (7) The finished product is obtained by cutting ...
Embodiment 2
[0034] Recipe 2:
[0035] Component Formula (wt%) 200 mesh coal gangue10 400 mesh slag40 Secondary fly ash20 Water glass (m=1.8)22 Coconut Fatty Acid Diethanolamide1.5 Aluminum powder foaming agent0.5 water8 total100
[0036] The preparation method is as follows:
[0037] (1) Prepare various raw materials in proportion;
[0038] (2) Mix coal gangue, slag, fly ash, and coconut fatty acid diethanolamide according to the proportions into powder material;
[0039] (3) Add modulus m=1.8 water glass and water to the mixed powder material and stir evenly to obtain slurry;
[0040] (4) Add the aluminum powder foaming agent to the slurry, mix and stir evenly, then pour it into the mold and foam it into a green body;
[0041] (5) Cut the cast body after 6 hours of static stop at room temperature.
[0042] (6) Put the cut plate into the autoclave for autoclave, the pressure is 8×Pa, the temperature is 175℃, and the autoclave time is 12h.
[0043] (7) The finished product is obtained by cut...
Embodiment 3
[0045] Formula Three:
[0046] Component Formula (wt%) 300 mesh coal gangue20 200 mesh slag20 Secondary fly ash30 Water glass (m=2.0)24 Mixture of calcium stearate and coconut fatty acid diethanolamide0.1 Aluminum powder foaming agent0.9 water5 total100
[0047] Preparation:
[0048] (1) Prepare various raw materials in proportion;
[0049] (2) Mix coal gangue, slag, fly ash, calcium stearate, and coconut fatty acid diethanolamide according to the proportions to make a powder material;
[0050] (3) Add modulus m=2.0 water glass and water to the mixed powder material and stir evenly to obtain slurry;
[0051] (4) Add the aluminum powder foaming agent to the slurry, mix and stir evenly, then pour it into the mold and foam it into a green body;
[0052] (5) Cut the cast body after 4 hours of static stop at room temperature.
[0053] (6) Put the cut plates into an autoclave for autoclave, the pressure is 9×Pa, the temperature is 190℃, and the autoclave time is 8h.
[0054] (7) The f...
PUM
Property | Measurement | Unit |
---|---|---|
modulus | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com