A cement floor coating
A technology of ground coating and cement, applied in the direction of coating, can solve the problems of poor water resistance and weather resistance, friction resistance, low bonding strength, etc., and achieve the effect of good wear resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0015] A kind of cement floor paint, its raw material ratio is as follows in parts by weight: 100 parts of acrylic resin; 1 part of methyl methacrylate; 45 parts of glass beads; 3 parts of methacrylic acid; 1 part of soybean lecithin; 10 parts of butyl ester; 5 parts of deionized water; 15 parts of hydroxyethyl acrylate; 20 parts of iron oxide yellow; 10 parts of ethyl methacrylate; 20 parts of cobalt octanoate; 15 parts of ethyl acrylate; dibutyl phthalate 25 parts; 15 parts of ethyl acetate; 30 parts of rosin; 35 parts of toluene.
[0016] After dissolving toluene in deionized water, add iron oxide yellow and soybean lecithin, mill with a ball mill for 30 minutes, add cobalt octanoate, acrylic resin, methyl methacrylate, glass beads, methacrylic acid and isobutyl methacrylate, Ball mill for 30 minutes, add hydroxyethyl acrylate and the remaining raw materials, and filter the finished product with gauze after ball milling for 1 hour.
[0017] Coating reciprocating testing ma...
Embodiment 2
[0019] A kind of cement floor paint, its raw material ratio is as follows by weight: 100 parts of acrylic resin; 10 parts of methyl methacrylate; 55 parts of glass beads; 5 parts of methacrylic acid; 5 parts of soybean lecithin; 20 parts of butyl ester; 15 parts of deionized water; 25 parts of hydroxyethyl acrylate; 30 parts of iron oxide yellow; 30 parts of ethyl methacrylate; 40 parts of cobalt octanoate; 25 parts of ethyl acrylate; dibutyl phthalate 35 parts; 35 parts of ethyl acetate; 40 parts of rosin; 45 parts of toluene.
[0020] After dissolving toluene in deionized water, add iron oxide yellow and soybean lecithin, mill with a ball mill for 30 minutes, add cobalt octanoate, acrylic resin, methyl methacrylate, glass beads, methacrylic acid and isobutyl methacrylate, Ball mill for 30 minutes, add hydroxyethyl acrylate and the remaining raw materials, and use gauze to filter the finished product after ball milling for 1 hour.
[0021] Coating reciprocating testing machi...
Embodiment 3
[0023] A kind of cement floor coating, its raw material ratio is as follows by weight: 100 parts of acrylic resin; 5 parts of methyl methacrylate; 50 parts of glass beads; 4 parts of methacrylic acid; 3 parts of soybean lecithin; 15 parts of butyl ester; 10 parts of deionized water; 20 parts of hydroxyethyl acrylate; 25 parts of iron oxide yellow; 20 parts of ethyl methacrylate; 30 parts of cobalt octanoate; 20 parts of ethyl acrylate; dibutyl phthalate 30 parts; 25 parts of ethyl acetate; 35 parts of rosin; 40 parts of toluene.
[0024] After dissolving toluene in deionized water, add iron oxide yellow and soybean lecithin, mill with a ball mill for 30 minutes, add cobalt octanoate, acrylic resin, methyl methacrylate, glass beads, methacrylic acid and isobutyl methacrylate, Ball mill for 30 minutes, add hydroxyethyl acrylate and the remaining raw materials, and use gauze to filter the finished product after ball milling for 1 hour.
[0025] Coating reciprocating testing mach...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com