Preparation method of granite polishing powder
A polishing powder and granite technology, which is applied in the direction of grinding/polishing equipment, polishing composition containing abrasives, manufacturing tools, etc., can solve the problem that the polishing of granite cannot achieve the polishing effect, and achieve particle size distribution The effect of narrow range, low production cost and simple preparation process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] A kind of preparation of granite polishing powder: in reactor, add the ammonium dichromate of 6g, 12g zirconium oxychloride is dissolved in water, then add the aluminum oxide of 58g, add the titanium dioxide of 8g, add 1.0 tensio-active agent, Stir to form a slurry, then add 15g of ammonium carbonate, stir to dissolve, the sum of each component is 100%, water is not included in the component, under normal pressure, stir, add heat at 70°C, and react for 25h, so that the zirconium oxychloride produces uniform particles Zirconium dioxide particles, evaporated to dryness, then raised the temperature to 190°C, reacted for 3 hours to make ammonium dichromate produce uniform chromium trioxide, roasted at 1100°C for 1.5 hours, cooled, and crushed by airflow to obtain Granite polishing powder.
Embodiment 2
[0024] A preparation of granite polishing powder: in the reactor, add 10g of ammonium dichromate, dissolve 6g of zirconium oxychloride in water, then add 69.5g of aluminum oxide, add 2g of titanium dioxide, add 0.5 surfactant , stir to form a slurry, then add 12g of ammonium carbonate, stir to dissolve, the sum of each component is 100%, water is not included in the component, under normal pressure, stir, add heat at 75°C, and react for 30h to make the particles of zirconium oxychloride uniform The zirconia particles were evaporated to dryness, and then the temperature was raised to 195°C, and reacted for 2 hours to make ammonium dichromate produce uniform chromium trioxide particles, roasted at 1100°C for 1 hour, and after cooling, they were pulverized by air flow to obtain Granite polishing powder.
Embodiment 3
[0026] A kind of preparation of granite polishing powder: in reactor, add the ammonium dichromate of 12g, 17g zirconium oxychloride is dissolved in water, then add the Al2O3 of 50g, add the titanium dioxide of 10g, add 1.0 tensio-active agent, Stir to form a slurry, then add 10g of ammonium carbonate, stir to dissolve, the sum of each component is 100%, water is not included in the component, under normal pressure, stir, add heat at 75°C, and react for 20h, so that the zirconium oxychloride produces uniform particles Zirconium dioxide particles, evaporated to dryness, then raise the temperature to 190°C, react for 4h, make ammonium dichromate produce uniform chromium trioxide, roast at 1000°C for 2.0h, after cooling, crush by airflow to obtain Granite polishing powder.
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
Mohs hardness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com