A water-based pigment, inkjet printing technology, applied in printing, ink, application, etc., can solve the problems of affecting the storage stability of ink, insufficient rubbing fastness, etc., and achieve good comprehensive physical properties of the picture, excellent sunlight resistance, printing Good fluency effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0032] Table 1 contains the water-based pigment type red ink formula of emulsion
[0033] components
Mass percentage (%)
C.I. Pigment Red 48:2
5.0
[0034] Dispersant BYK190
3.8
0.2
1.0
2-pyrrolidone
5.0
1,3-propanediol
7.0
1,4-Butanediol
3.2
Polyethylene glycol 600
1.8
Tween 85
0.4
1.0
Emulsion SD-688
19.0
Deionized water
52.6
[0035] Note: BYK190 is a water-based dispersant, provided by BYK Chemical Technology Consulting (Shanghai) Co., Ltd.
[0036] According to the ratio in Table 1, add dispersant BYK190, fungicide s-triazine and propylene glycol into deionized water, disperse with emulsifier for 55 minutes, then add C.I. Pigment Red 48:2, continue to disperse for 35 minutes, then use sand mill The machine grinds at 4000rad / min f...
Embodiment 2
[0038] Table 2 contains the water-based pigment type yellow ink formula of emulsion
[0039] components
[0040] dipropylene glycol propyl ether
[0041] According to the ratio in Table 2, add dispersant BYK190 and ethylene glycol into deionized water, disperse with an emulsifier for 55 minutes, then add C.I. Pigment Yellow 87, and continue to disperse for 35 minutes. Then use a sand mill to grind for 20 hours at a speed of 4000 rad / min and then take it out to obtain a yellow pigment dispersion. Then, the surfactant, film-forming aid, the remaining amount of water-soluble co-solvent and deionized water are stirred and mixed with a mixer at a speed of 800rad / min for 30min at room temperature, and then the emulsion HD2083 is slowly added to the mixed solution, and the stirring is continued. 30min. Slowly add the pigment dispersion while stirring, and continue stirring for 90 minutes. After the various components are fully mixed to form a uniform dispersion ...
Embodiment 3
[0043] Table 3 contains the water-based pigment type blue ink formula of emulsion
[0044] components
Mass percentage (%)
C.I. Pigment Blue 15:3
5.0
Dispersant SP-724
2.0
0.2
5.0
2-pyrrolidone
1.8
[0045] Diethylene glycol
6.0
1,6-Hexanediol
4.0
Span 80
1.6
Tween 40
0.5
Emulsion MW-713
16.0
Deionized water
57.9
[0046] Note: SP-724 is a water-based dispersant, purchased from Dongguan Bocheng Chemical Co., Ltd.
[0047] According to the formula in Table 3, add dispersant SP-724 and fungicide s-triazine into deionized water, emulsify with emulsifier for 45min, then add C.I. After grinding for 6 hours at a rotating speed, take it out to obtain a blue pigment dispersion. Mix the surfactant, film-forming aid and the remaining water-soluble co-solvent evenly at room temperature, stir for 15 ...
PUM
Property | Measurement | Unit |
---|---|---|
glass transition temperature | aaaaa | aaaaa |
glass transition temperature | aaaaa | aaaaa |
surface tension | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com