Waterborne polyurethane resin superfiber leather and manufacturing method thereof
A technology of superfine fiber leather and water-based polyurethane, which is applied in the field of polyurethane resin synthetic leather and synthetic leather and manufacturing, to achieve the effects of reducing environmental pollution, reducing product cost and superior performance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0045] Nylon-6 and alkali-soluble polyester are mixed and melt-spun in a ratio of 8:2. The two raw materials are melted, mixed, and extruded in an extruder to form a sea-island structure filament in which nylon-6 is an island and alkali-soluble polyester is a sea. Let the stretched monofilament be 10-15 denier. Perform 2 extensions at 180-220 degrees, and the extension rate is 3.0-4.0 times. The multi-component mixed spinning fiber of the present invention can reach 3-5 denier by stretching, and the sea-island fiber is crimped by machinery and cut into 51mm long fiber. The sea-island fiber is carded into a net and laid into 250-300g / m 2 The cotton net is needle-punched and PVA heat-fixed to form the original fabric for processing. After wet processing such as polyurethane resin dipping and coating, after the polyurethane resin is thermally solidified, the sea-island fiber is removed by alkali reduction treatment to form a superfine fiber structure. The base fabric is inspe...
Embodiment 2
[0049] Nylon-6 and alkali-soluble polyester are mixed and melt-spun in a ratio of 7:3. The two raw materials are melted, mixed, and extruded in an extruder to form a sea-island structure filament in which nylon-6 is an island and alkali-soluble polyester is a sea. Let the stretched monofilament be 10-15 denier. Perform 2 extensions at 50-95 degrees, and the extension rate is 2.5-4.0 times. The multi-component mixed spinning fiber of the present invention can reach 4-8 denier by stretching, and the sea-island fiber is crimped by machinery and cut into 51mm long fiber. The sea-island fiber is carded into a net and laid into 350-450g / m 2 The cotton net is needle-punched and PVA heat-fixed to form the original fabric for processing. After wet processing such as polyurethane resin dipping and coating, after the polyurethane resin is thermally solidified, the sea-island fiber is removed by alkali reduction treatment to form a superfine fiber structure.
[0050] The water-based p...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com