Embodiment 1
[0069] This embodiment provides a spray-type colored asphalt, the composition of raw materials is as follows:
[0070]
[0071] Spray type colored asphalt preparation method:
[0072] (1) Add the oil extracted from the third line and C5 petroleum resin into the asphalt modification tank, heat up to 160°C and stir for 1 hour to mix evenly, then heat up to 180°C and add SBS to cut, cut for 1.5 hours, keep the temperature constant, Add 1 part of toner, stir for 0.5h to mix evenly;
[0073] (2) Add ethyl acetate into the mixing tank, slowly add the melted colored asphalt into the mixing tank and keep stirring, the temperature is controlled at 40°C, stir for 2 hours to disperse evenly, then add No. 120 solvent naphtha and keep stirring, Control the temperature at 30°C, stir for 1 hour to disperse evenly;
[0074] (3) Add the dolomite powder into the uniformly dispersed solvent, stir and mix at room temperature for 0.5h to mix evenly, and prepare the spray-type colored asphalt....
Embodiment 2
[0076] This embodiment provides a spray-type colored asphalt, the composition of raw materials is as follows:
[0077]
[0078] Spray type colored asphalt preparation method:
[0079] (1) Add the oil extracted from the third line and C5 petroleum resin into the asphalt modification tank, heat up to 160°C and stir for 1 hour to mix evenly, then heat up to 180°C and add SBS to cut, cut for 1.5 hours, keep the temperature constant, Add 1 part of toner, stir for 0.5h to mix evenly;
[0080] (2) Add methyl acetate into the mixing tank, slowly add the melted colored pitch into the mixing tank and keep stirring, the temperature is controlled at 40°C, stir for 2h to disperse evenly, then add cyclohexane and keep stirring, the temperature Control at 30°C, stir for 1 hour to disperse evenly;
[0081] (3) Add the limestone powder into the uniformly dispersed solvent, stir and mix at room temperature for 0.5h to mix evenly, and prepare the spray-type colored asphalt.
Embodiment 3
[0083] This embodiment provides a spray-type colored asphalt, the composition of raw materials is as follows:
[0084]
[0085]
[0086] Spray type colored asphalt preparation method:
[0087] (1) Add aromatic oil and C9 petroleum resin into the asphalt modification tank, heat up to 160°C and stir for 1 hour to mix evenly, then heat up to 180°C and add SBS to cut, cut for 1.5 hours, keep the temperature unchanged, add color 1 part of powder, stir for 0.5h to mix evenly;
[0088] (2) Add ethyl acetate into the mixing tank, slowly add the melted colored asphalt into the mixing tank and keep stirring, the temperature is controlled at 40°C, stir for 2 hours to disperse evenly, then add No. 140 solvent naphtha and keep stirring, Control the temperature at 30°C, stir for 1 hour to disperse evenly;
[0089] (3) Add talc powder and mineral powder into the uniformly dispersed solvent, stir and mix at room temperature for 0.5h to mix evenly, and prepare spray-type colored asphal...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com