Gold/oxide catalyst and application in preparing DHA through catalytic oxidation of glycerol
A technology of oxides and catalysts, applied in gold/oxide catalysts and in the application field of catalytic oxidation of glycerol to prepare DHA, can solve the problems of no research on gold catalysts, achieve good industrial prospects, and the preparation method is simple and easy to operate, and the reaction conditions mild effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0028] The gold / oxide catalyst of the present embodiment is prepared by the following method:
[0029] (1) Take 6 g of lilac leaf powder in 100 mL of water, stir at 30° C. for 6 h, then centrifuge and filter to obtain a water extract, freeze-dry the water extract to obtain a lilac leaf extract;
[0030] (2) 12.08g Cu(NO 3 ) 2 ·3H 2 O was dissolved in 200 mL of deionized water while adding 1M Na 2 CO 3 Adjust the pH to 10, then place the mixed solution at room temperature and stir for 12 hours; filter and wash the resulting mixed solution to neutrality, and dry the filter cake in a vacuum oven at 60°C for 24 hours. 2 Under the atmosphere, the temperature was raised to 350°C for 4 hours at a rate of 2°C / min to obtain a CuO carrier;
[0031] (3) Take 0.99g CuO carrier in 50mL deionized water, then add 1.04mL 48.56mM chloroauric acid solution, stir at 30°C for 4h, continue to add 100mg of lilac leaf extract, stir for 4h; pump the obtained material Filter and wash until free ...
Embodiment 2
[0036] The gold / oxide catalyst of the present embodiment is prepared by the following method:
[0037] (1) Take 6 g of lilac leaf powder in 100 mL of water, stir at 30° C. for 6 h, then centrifuge and filter to obtain a water extract, freeze-dry the water extract to obtain a lilac leaf extract;
[0038] (2) 12.08g Cu(NO 3 ) 2 ·3H 2 O was dissolved in 200 mL of deionized water while adding 1M Na 2 CO 3 Adjust the pH to 10, then place the mixed solution at room temperature and stir for 12 hours; filter and wash the resulting mixed solution to neutrality, and dry the filter cake in a vacuum oven at 60°C for 24 hours. 2 Under the atmosphere, the temperature was raised to 350°C for 4 hours at a rate of 2°C / min to obtain a CuO carrier;
[0039] (3) Take 0.99g CuO carrier in 50mL deionized water, then add 1.04mL 48.56mM chloroauric acid solution, stir at 30°C for 4h, continue to add 200mg of lilac leaf extract, stir for 4h; pump the obtained material Filter and wash until free ...
Embodiment 3
[0043] The gold / oxide catalyst of the present embodiment is prepared by the following method:
[0044](1) Take 6g of the powder of Peach leaves in 100mL of water, stir at 30°C for 6h, then centrifuge and filter to obtain a water extract, freeze-dry the water extract to obtain a Peach leaf extract;
[0045] (2) 12.08g Cu(NO 3 ) 2 ·3H 2 O was dissolved in 200 mL of deionized water while adding 1M Na 2 CO 3 Adjust the pH to 10, then place the mixed solution at room temperature and stir for 12 hours; filter and wash the resulting mixed solution to neutrality, and dry the filter cake in a vacuum oven at 60°C for 24 hours. 2 Under the atmosphere, the temperature was raised to 350°C for 4 hours at a rate of 2°C / min to obtain a CuO carrier;
[0046] (3) Take 0.99g CuO carrier in 50mL deionized water, then add 1.04mL 48.56mM chloroauric acid solution, stir at 30°C for 4h, continue to add 100mg of Peach leaf extract, stir for 4h; filter the resulting material Wash until free of ch...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com