[0021] A water-based paint for golden nanmu furniture, which consists of the following components in parts by weight: 60 parts of water-soluble resin, 20 parts of acrylic acid, 18 parts of polyethylene glycol, 23 parts of modified nano-silica, and 20 parts of modified plateau soil , 5 parts of nano zinc oxide, 9 parts of lanthanum carbonate, 8 parts of sodium carbonate, 6 parts of cerium nitrate, 5 parts of phenylethyl alcohol oleate, 3 parts of polyoxypropylene glyceryl ether, 10 parts of sodium alginate, 40 parts of sterile water.
[0022] Further, the preparation of the modified nano silicon dioxide comprises the following steps:
[0023] 1) Put the nano-silica and the modified solution A in the reactor at a weight ratio of 1:5, control the temperature in the reactor to 300°C, control the pressure in the reactor to 10MPa, and stir for 40 minutes;
[0024] 2) When the temperature in the reaction kettle in operation 1) drops to room temperature, take out the nano-silica and p...
Embodiment 2
[0032] A water-based paint for golden nanmu furniture, which consists of the following components in parts by weight: 65 parts of water-soluble resin, 22 parts of acrylic acid, 19 parts of polyethylene glycol, 24 parts of modified nano-silica, and 23 parts of modified plateau soil , 5.5 parts of nano-zinc oxide, 11 parts of lanthanum carbonate, 10 parts of sodium carbonate, 8 parts of cerium nitrate, 7 parts of phenylethyl alcohol oleate, 4 parts of polyoxypropylene glyceryl ether, 13 parts of sodium alginate, and 45 parts of sterile water.
[0033] Further, the preparation of the modified nano silicon dioxide comprises the following steps:
[0034] 1) Put the nano-silica and the modified liquid A together in the reactor according to the weight ratio of 1:5.5. The temperature in the reactor is controlled at 350°C, the pressure in the reactor is controlled at 15MPa, and the stirring process is carried out for 45 minutes;
[0035] 2) When the temperature in the reaction kettle i...
Embodiment 3
[0043] A water-based paint for golden nanmu furniture, which is composed of the following components in parts by weight: 70 parts of water-soluble resin, 24 parts of acrylic acid, 20 parts of polyethylene glycol, 25 parts of modified nano-silica, and 26 parts of modified plateau soil , 6 parts of nano zinc oxide, 13 parts of lanthanum carbonate, 12 parts of sodium carbonate, 10 parts of cerium nitrate, 9 parts of phenylethyl alcohol oleate, 5 parts of polyoxypropylene glyceryl ether, 16 parts of sodium alginate, and 50 parts of sterile water.
[0044] Further, the preparation of the modified nano silicon dioxide comprises the following steps:
[0045] 1) Put the nano-silica and the modified solution A in the reactor at a weight ratio of 1:6, control the temperature in the reactor to 400°C, control the pressure in the reactor to 20MPa, and stir for 50 minutes;
[0046] 2) When the temperature in the reaction kettle in operation 1) drops to room temperature, take out the nano-si...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com