Polyolefin composite material and preparation method thereof
A composite material and polyolefin technology, applied in the field of polyolefin composite materials, can solve problems such as unacceptable, odor overflow, and long-term performance attenuation of materials, and achieve the effects of optimizing, reducing, and promoting elimination
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0034] The preparation method of a kind of polyolefin composite material of present embodiment, the steps are as follows:
[0035] (1) Take 130g polyethylene, 10g POE, 60g talcum powder, 0.2g primary antioxidant 1076 and 0.2g secondary antioxidant 168, and blend these compounds uniformly to obtain a mixture;
[0036] (2) Add the mixture into a microwave reaction tank, set the microwave reaction power to 1000W, microwave frequency to 250000MHz, and microwave to heat to 200°C for 200s; after the reaction, cool to obtain a polyethylene composite material.
Embodiment 2
[0053] The preparation method of a kind of polyolefin composite material of present embodiment, the steps are as follows:
[0054] (1) Get 130g polypropylene, 10gPOE, 60g calcium carbonate, 0.4g primary antioxidant 1010 and 0.4g secondary antioxidant 626, and blend these compounds uniformly to obtain a mixture;
[0055] (2) Add the mixture into a microwave reaction tank, set the microwave reaction power to 3000W, microwave frequency to 50000MHz, and microwave heating to 250°C for 400s; after the reaction, cool to obtain a polypropylene composite material.
[0056] After the odor evaluation of the above polypropylene composite material, the odor grade is 2.6.
Embodiment 3
[0063] The preparation method of a kind of polyolefin composite material of present embodiment, the steps are as follows:
[0064] (1) Get 100g polybutene, 80gPOE, 20g wollastonite, 1.0g primary antioxidant 1790 and 1.0g secondary antioxidant DLTP, and blend these compounds uniformly to obtain a mixture;
[0065] (2) Add the mixture into a microwave reaction tank, set the microwave reaction power to 6000W, microwave frequency to 800MHz, and microwave heating to 230°C for 80s; after the reaction, cool to obtain a polybutene composite material.
[0066] After carrying out the odor evaluation to the above polybutene composite material, the odor rating is 2.7.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com