Preparation method for elastic plastic and wood composite floor surface course material with insect prevention effect
A compound floor and elastic technology, applied in the field of wood-plastic floor, can solve the problems of human hazards, poor ventilation effect, chemical component residue, etc., and achieve the effect of increasing the duration, good insect repellent effect, and improved insect repellent effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0040] A method for preparing an elastic wood-plastic composite floor surface material with an insect-proof effect is carried out according to the following steps:
[0041] A. Put each raw material into a high-speed mixer for mixing, the temperature is 100°C, the mixing time is 12min, and the mixing speed is 1120rpm;
[0042] B. In the third step, the mixed material is granulated by a special granulator; the temperature is 175°C, and the screw speed is 220rpm;
[0043] C. Use an extruder to extrude the granulated material into shape, and the extrusion temperature is 170°C.
[0044] The raw material in the described step A comprises the composition of following percentage by weight:
[0045] TPE 36%
[0046] Wood flour 10%
[0047] Maleic anhydride grafted polyethylene 2%
[0048] Lubricant 1%
[0049] Antioxidant 0.5%
[0050] UV absorber 0.5%
[0051] Natural Plant Modified Insect Repellent 1.5%
[0052] HDPE allowance.
[0053] The particle size of the wood flour is...
Embodiment 2
[0060] A method for preparing an elastic wood-plastic composite floor surface material with an insect-proof effect is carried out according to the following steps:
[0061] A. Put each raw material into a high-speed mixer for mixing, the temperature is 80°C, the mixing time is 15min, and the mixing speed is 1000rpm;
[0062] B. In the third step, the mixed material is granulated by a special granulator; the temperature is 180°C, and the screw speed is 150rpm;
[0063] C. Use an extruder to extrude the granulated material into shape, and the extrusion temperature is 180°C.
[0064] The raw material in the described step A comprises the composition of following percentage by weight:
[0065] TPE (elastic polyethylene) 30%
[0066] Wood flour 12%
[0067] Maleic anhydride grafted polyethylene 1.5%
[0068]Lubricant 1.5%
[0069] Antioxidant 0.3%
[0070] UV absorber 0.6%
[0071] Natural Plant Modified Insect Repellent 1%
[0072] HDPE (High Density Polyethylene) balance....
Embodiment 3
[0080] A method for preparing an elastic wood-plastic composite floor surface material with an insect-proof effect is carried out according to the following steps:
[0081] A. Put each raw material into a high-speed mixer for mixing, the temperature is 120°C, the mixing time is 10min, and the mixing speed is 1200rpm;
[0082] B. In the third step, the mixed material is granulated by a special granulator; the temperature is 160°C, and the screw speed is 300rpm;
[0083] C. Use an extruder to extrude the granulated material into shape, and the extrusion temperature is 160°C.
[0084] The raw material in the described step A comprises the composition of following percentage by weight:
[0085] TPE (elastic polyethylene) 40%
[0086] Wood flour 8%
[0087] Maleic anhydride grafted polyethylene 2.5%
[0088] Lubricant 0.8%
[0089] Antioxidant 0.6%
[0090] UV absorber 0.3%
[0091] Natural Plant Modified Insect Repellent 2%
[0092] HDPE (High Density Polyethylene) balance...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com