Quick-drying wax oil and preparation method thereof
A wood wax oil and drying technology, applied in the field of coatings, can solve the problems of high energy consumption, high viscosity, and high cost, and achieve the effects of saving energy and time, good moisture permeability, and reducing preparation costs
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0033] A quick-drying wood wax oil, in parts by weight, consists of the following components:
[0034] JC116 alkyd resin 45%, 1105 alkyd resin 15%, carnauba wax 3.5%, candelilla wax 5%, beeswax 1.5%, fatty acid methyl ester 5%, 8% cobalt isooctanoate 0.05%, 8% manganese isooctanoate 0.05%, LC-801 rare earth drier 0.5%, D-limonene solvent naphtha 15%, D40 solvent naphtha 9.3%, BHT antioxidant 0.1%.
[0035] A preparation method for quick-drying wood wax oil, comprising the following steps:
[0036] (1) Put JC116 alkyd resin, 1105 alkyd resin, carnauba wax, candelilla wax, beeswax, and fatty acid methyl ester into the reaction kettle in proportion, disperse at 80°C and 800r / min, keep the temperature for 30 minutes and then drop to room temperature;
[0037] (2) Add 8% cobalt isooctanoate, 8% manganese isooctanoate, LC-801 rare earth drier, D-limonene solvent oil, D40 solvent oil, and BHT antioxidant to the cooled reactant in proportion, at 30°C , 600r / min disperse for 10 minu...
Embodiment 2
[0041] A quick-drying wood wax oil, in parts by weight, consists of the following components:
[0042] JC116 alkyd resin 48%, 1105 alkyd resin 16%, carnauba wax 3%, candelilla wax 4%, beeswax 1%, fatty acid methyl ester 4.5%, cobalt naphthalate 0.06%, manganese naphthalate 0.06%, LC -801 rare earth drier 0.4%, D-limonene solvent naphtha 22.93%, BHT antioxidant 0.05%.
[0043] A preparation method for quick-drying wood wax oil, comprising the following steps:
[0044] (1) Put JC116 alkyd resin, 1105 alkyd resin, carnauba wax, candelilla wax, beeswax, and fatty acid methyl ester into the reaction kettle in proportion, disperse at 78°C and 1200r / min, keep the temperature for 30 minutes and then drop to room temperature;
[0045] (2) Add cobalt naphthenate, manganese naphthenate, LC-801 rare earth drier, D-limonene solvent oil, and BHT antioxidant to the reactant after cooling down in proportion, and disperse at 40°C and 550r / min for 10 minutes. It is well mixed;
[0046] (3) ...
Embodiment 3
[0048] A quick-drying wood wax oil, in parts by weight, consists of the following components:
[0049] JC116 alkyd resin 42%, 1105 alkyd resin 14%, carnauba wax 4%, candelilla wax 6%, beeswax 2%, fatty acid methyl ester 5.5%, 8% cobalt isooctanoate 0.04%, 8% manganese isooctanoate 0.04%, LC-801 rare earth drier 0.6%, D-limonene solvent naphtha 25.67%, BHT antioxidant 0.15%.
[0050] A preparation method for quick-drying wood wax oil, comprising the following steps:
[0051] (1) Put JC116 alkyd resin, 1105 alkyd resin, carnauba wax, candelilla wax, beeswax, and fatty acid methyl ester into the reaction kettle in proportion, disperse at 79°C and 800r / min, keep the temperature for 30 minutes and then drop to room temperature;
[0052] (2) Add 8% cobalt isooctanoate, 8% manganese isooctanoate, LC-801 rare earth drier, D-limonene solvent oil, and BHT antioxidant to the cooled reactant in proportion, 50°C, 500r / min Disperse for 10 minutes to make it evenly mixed;
[0053] (3) Ch...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com