manufacture Embodiment 1-9
[0282]
[0283] For the cleaning blade, an elastomer blade made of polyurethane is dipped in an isocyanate-based treatment liquid to adjust the surface friction coefficient and surface elastic modulus.
[0284] Specifically, an elastomer blade made of polyurethane is dipped in a treatment liquid obtained by dissolving at least one selected from a fluorine-based polymer and a silicon-based polymer and added to an isocyanate component in a solvent and Properly refined. Elastomeric blades having physical properties shown in Table 1 below were manufactured by changing the addition amounts of the isocyanate component, fluorine-based polymer, and silicon-based polymer to thereby change the concentration of the treatment liquid.
[0285] [Table 1]
[0286]
[0287] The unit of surface elastic modulus is N / mm 2 .
[0288] ~Manufacture of toner~
[0289]
[0290] Sodium lauryl sulfate (0.7 parts) and ion-exchanged water (498 parts) were placed in a reaction vessel equipped w...
manufacture Embodiment 10
[0320]
[0321] As the cleaning blade of Manufacturing Example 10, the elastomer blade described in Example 2 in JP-A No. 2010-210879 was used as it was. That is, the elastomer blade of Example 10 was produced as follows.
[0322] -Urethane rubber
[0323] Urethane rubber having hardness of 69° and impact resilience of 49% (manufactured by Toyo Tire & Rubber Co., Ltd.)
[0324] The hardness of the urethane rubber was measured according to JIS K6253 with a durometer manufactured by Shimadzu Corporation. The sample is a laminate having a thickness of 6 [mm] or more obtained by laminating sheets having a thickness of about 2 [mm].
[0325] The impact resilience of the urethane rubber was measured with a RESILIENCE TESTER No. 221 manufactured by Toyo Seiki Seisaku-Sho, Ltd. according to JIS K6255. The sample is a laminate having a thickness of 4 [mm] or more obtained by laminating sheets having a thickness of about 2 [mm]. - Dipping solution
[0326] Isocyanate compound: MR...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com