A technology of reforming protective agent and extrusion aid, which is applied in the direction of reforming naphtha, chemical instruments and methods, molecular sieve catalysts, etc., and can solve the problem of small catalyst pore size and specific surface area, uneven distribution of active components, and long service life of catalysts. Short and other problems, to avoid side reactions, long service life, improve the effect of mechanical strength
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0039] This embodiment provides a reforming protective agent whose raw material composition includes:
[0040] Acidified pseudo-boehmite, 15 parts by weight;
[0041] Acidified Y type molecular sieve, 25 parts by weight;
[0042] Manganese carbonate, 25 parts by weight;
[0043] Ferric hydroxide, 33 parts by weight;
[0044] Synthetic methanol catalyst waste agent, 38 parts by weight;
[0045] Squeezing aid silica sol, 50 parts by weight.
[0046] Wherein, the acidified pseudo-boehmite is prepared by the following method:
[0047] 100 parts by weight of pseudo-boehmite and 120 parts by weight of 10 wt% nitric acid solution were formed into a gel at 55° C. and mixed uniformly.
[0048] The acidified molecular sieve is prepared by the following method:
[0049] Mix 100 parts by weight of molecular sieve with 95 parts by weight of 5 wt% acetic acid solution, add 100 parts by weight of 25% aluminum sol to make it colloidal, and dry at 100°C.
[0050] Described synthetic metha...
Embodiment 2
[0058] This embodiment provides a reforming protective agent whose raw material composition includes:
[0059] Acidified pseudo-boehmite, 10 parts by weight;
[0060] Acidified β-type molecular sieve, 45 parts by weight;
[0061] Manganese oxide, 15 parts by weight;
[0062] Iron oxide red, 40 parts by weight;
[0063] Synthetic methanol catalyst waste agent, 15 parts by weight;
[0064] Extrusion aid aluminum sol, 50 parts by weight.
[0065] Wherein, the acidified pseudo-boehmite is prepared by the following method:
[0066] 100 parts by weight of pseudo-boehmite and 80 parts by weight of 20 wt% nitric acid solution were formed into a gel at 55° C. and mixed uniformly.
[0067] The acidified molecular sieve is prepared by the following method:
[0068] Mix 100 parts by weight of molecular sieve with 120 parts by weight of 15 wt% acetic acid solution, add 100 parts by weight of 22% aluminum sol to make it colloidal, and dry at 100°C.
[0069] Described synthetic methan...
Embodiment 3
[0077] This embodiment provides a reforming protective agent whose raw material composition includes:
[0078] Acidified pseudo-boehmite, 25 parts by weight;
[0079] Acidified MCM type molecular sieve, 20 parts by weight;
[0080] The mixture of manganese oxide and manganese carbonate with a mass ratio of 1:1, 30 parts by weight;
[0081] Red mud, 20 parts by weight;
[0082] Synthetic methanol catalyst waste agent, 40 parts by weight;
[0083] Extrusion aid carboxymethyl cellulose, 30 parts by weight.
[0084] Wherein, the acidified pseudo-boehmite is prepared by the following method:
[0085] 100 parts by weight of pseudo-boehmite and 135 parts by weight of 12 wt% nitric acid solution were formed into a gel at 55° C. and mixed uniformly.
[0086] The acidified molecular sieve is prepared by the following method:
[0087] Mix 100 parts by weight of molecular sieve with 140 parts by weight of 10 wt% acetic acid solution, add 100 parts by weight of 29% aluminum sol to ma...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com