Copper alloy for precision casting of artwork, and preparation method and method for precision casting
A technology of precision casting and artwork, applied in casting molding equipment, metal processing equipment, casting molds, etc., can solve the problems of restricting the progress of cultural artworks, not suitable for precision forging, increasing production costs, etc., and achieve the reduction of mechanical properties and flow The effect of increasing resistance and reducing burning loss
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0054] A method for processing copper alloys for precision casting of works of art, the steps are:
[0055] (1) First add Cu with a mass fraction of 47.0% into the crucible to melt and heat to 1098°C;
[0056] (2) Grinding Fe with a mass fraction of 1.5% into a powder with a diameter of 9-15nm for later use;
[0057] (3) Sb film with a mass fraction of 3.7% is made into a Sb film with a thickness of 0.3mm, and Te powder with a mass fraction of 0.3% is wrapped with the Sb film, and the particle size of the Te powder is 5-10nm;
[0058] (4) Add Bi with a mass fraction of 3.5%, Ni with a mass fraction of 1.0%, and Fe powder in step (2) to the crucible in step (1) in sequence, and when heated to 1105°C, add Zn and keep the temperature No change, stop heating after the Zn is completely melted, and immediately put the Sb film wrapped with Te powder obtained in step (3) to obtain the alloy melt;
[0059] (5) Cool the melt obtained in step (4) in air at a cooling rate equal to 15°C ...
Embodiment 2
[0062] Same as Example 1, the difference is: its composition and mass percentage content are: Cu: 45.0, Sb: 3.9%, Fe: 1.3, Bi: 4.0%, Ni: 0.5%, Te: 0.5%, and the balance is Zn ; The cooling rate per second in step (5) is equal to 13°C. The fluidity of this alloy is 114mm.
Embodiment 3
[0064] Same as Example 1, the difference is: its composition and mass percentage content are: Cu: 49.0%, Sb: 3.5%, Fe: 1.7%, Bi: 3.0%, Ni: 1.5%, Te: 0.2%, the balance is Zn; the cooling rate per second in step (5) is equal to 13°C. The fluidity of this alloy is 115mm.
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
thickness | aaaaa | aaaaa |
fluidity | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com