Rapid hemostatic dressing and preparation method thereof
A hemostatic dressing, fast technology, applied in medical science, absorbent pads, bandages, etc., can solve the problem that the hemostatic dressing is not suitable for rapid hemostasis, and achieve the effect of promoting blood aggregation, promoting wound healing, and promoting wound healing
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0031] The rapid hemostatic dressing of this embodiment includes the following raw material components in parts by weight: 30 parts of chitosan, 16 parts of sodium heparin, 10 parts of collagen, and 45 parts of aloin.
[0032] Its preparation method is:
[0033] (1) Mixing: mix chitosan, heparin sodium, collagen and aloin according to the selected parts by weight;
[0034] (2) Foaming treatment: place the above raw material mixture under vacuum at a temperature of 100°C for heating and foaming treatment for 3 hours;
[0035] (3) Aging: Cool the raw materials obtained in step (2) at room temperature to obtain a hemostatic cotton sheet;
[0036] (4) Wash the hemostatic cotton sheet obtained in step (3) with distilled water, process it into the desired shape, dry and sterilize it.
Embodiment 2
[0038] The rapid hemostatic dressing of this embodiment includes the following raw material components in parts by weight: 100 parts of chitosan, 30 parts of heparin sodium, 80 parts of collagen, and 10 parts of aloin.
[0039] Its preparation method is:
[0040] (1) Mixing: mix chitosan, heparin sodium, collagen and aloin according to the selected parts by weight;
[0041] (2) Foaming treatment: place the above raw material mixture under vacuum at a temperature of 200°C for heating and foaming treatment for 1 hour;
[0042] (3) Aging: Cool the raw materials obtained in step (2) at room temperature to obtain a hemostatic cotton sheet;
[0043] (4) Wash the hemostatic cotton sheet obtained in step (3) with distilled water, process it into the desired shape, dry and sterilize it.
Embodiment 3
[0045] The rapid hemostatic dressing of this embodiment includes the following raw material components in parts by weight: 65 parts of chitosan, 2 parts of sodium heparin, 45 parts of collagen, and 80 parts of aloin.
[0046] Its preparation method is:
[0047] (1) Mixing: mix chitosan, heparin sodium, collagen and aloin according to the selected parts by weight;
[0048] (2) Foaming treatment: place the above raw material mixture under vacuum at a temperature of 150°C for heating and foaming treatment for 1 hour;
[0049] (3) Aging: Cool the raw materials obtained in step (2) at room temperature to obtain a hemostatic cotton sheet;
[0050](4) Wash the hemostatic cotton sheet obtained in step (3) with distilled water, process it into the desired shape, dry and sterilize it.
PUM
Property | Measurement | Unit |
---|---|---|
Particle size | aaaaa | aaaaa |
Particle size | aaaaa | aaaaa |
Particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com