Preparation method of bonding agent for blast furnace stemming with good opening performance
A binder and blast furnace technology, which is applied in the field of blast furnace clay, can solve the problems of poor opening performance and complicated production process of the blast furnace clay, and achieve the effect of low production cost, good opening performance and not easy to agglomerate
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] A binder for blast furnace mud with good opening performance in this embodiment, each component is composed of the following parts by mass: 40 parts of asphalt, 6 parts of hydrogenated terphenyl, 10 parts of silicone resin, 11 parts of furan resin, and melamine formaldehyde resin 11 servings. Among them, the furan resin is furfuryl alcohol resin; the asphalt is petroleum asphalt, and the asphaltenes in the petroleum asphalt can be 25% to 30%.
[0025] A method for preparing a binder for blast furnace clay with good opening performance of the present embodiment, the steps are:
[0026] (1) Weigh 40 parts of asphalt and 6 parts of hydrogenated terphenyl in parts by mass, add the asphalt and hydrogenated terphenyl to the reaction kettle in turn, and stir and mix at a temperature of 55°C for 20 minutes;
[0027] (2) Weigh 10 parts of silicone resin, 11 parts of furan resin and 11 parts of melamine formaldehyde resin in parts by mass. Control the heating rate of the reactor...
Embodiment 2
[0029] A binder for blast furnace clay with good opening performance in this embodiment, each component is composed of the following parts by mass: 50 parts of asphalt, 4 parts of hydrogenated terphenyl, 12 parts of silicone resin, 8 parts of furan resin, and melamine formaldehyde resin 15 servings.
[0030] A method for preparing a binder for blast furnace clay with good opening performance of the present embodiment, the steps are:
[0031] (1) Weigh 50 parts of asphalt and 4 parts of hydrogenated terphenyl in parts by mass, add the asphalt and hydrogenated terphenyl to the reaction kettle in turn, and stir and mix at a temperature of 60°C for 20 minutes;
[0032] (2) Weigh 12 parts of silicone resin, 8 parts of furan resin and 15 parts of melamine formaldehyde resin in parts by mass, and control the heating rate of the reactor in step (1) to 4°C / min. When the temperature of the reactor reaches 76°C Finally, sequentially add silicone resin, furan resin and melamine formaldeh...
Embodiment 3
[0034] A binder for blast furnace clay with good opening performance in this embodiment, each component is composed of the following parts by mass: 45 parts of asphalt, 5 parts of hydrogenated terphenyl, 11 parts of silicone resin, 9 parts of furan resin, and melamine formaldehyde resin 13 servings.
[0035] A method for preparing a binder for blast furnace clay with good opening performance of the present embodiment, the steps are:
[0036] (1) Weigh 45 parts of asphalt and 5 parts of hydrogenated terphenyl in parts by mass, add the asphalt and hydrogenated terphenyl to the reaction kettle in turn, and stir and mix at a temperature of 58°C for 20 minutes;
[0037] (2) Weigh 11 parts of silicone resin, 9 parts of furan resin and 13 parts of melamine formaldehyde resin in parts by mass. Control the heating rate of the reactor in step (1) to 3.5°C / min. When the temperature of the reactor reaches 74°C Finally, sequentially add silicone resin, furan resin and melamine formaldehyd...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction