Hydrofining catalyst and preparation method thereof

A hydrofining and catalyst technology, applied in chemical instruments and methods, metal/metal oxide/metal hydroxide catalysts, physical/chemical process catalysts, etc. High active temperature and other problems, to achieve the effect of preventing grain fusion and growth, improving heat resistance, and low active temperature

Active Publication Date: 2013-01-09
CHINA PETROLEUM & CHEM CORP
View PDF3 Cites 39 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0004] However, it has been found in practice that these catalysts require a high activation temperature, generally between 280 and 290°C, and the aromatics in the material are also likely to participate in the reaction during high-temperature hydrogenation, resulting in the saturation of some aromatics and affecting the economic benefits of subsequent aromatics extraction.
For example, the active ingredient of the second-stage LY-8602 catalyst for pyrolysis gasoline used in industry is MoO 3 , CoO, the carrier is γ-Al 2 o 3 , in practical industrial applications, the catalyst has poor activity in hydrogenation of saturated monoolefins, and cannot adapt to the industrial conditions of heavy hydrogenation feedstock, variable sulfur content, higher and higher space velocity of hydrogenation liquid, and high service temperature (Reactor inlet temperature above 280°C), at this temperature, the hydrogenation loss of aromatics is high

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Hydrofining catalyst and preparation method thereof
  • Hydrofining catalyst and preparation method thereof
  • Hydrofining catalyst and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0027] A hydrorefining catalyst is prepared through the following steps:

[0028] Preparation of the carrier: 72.0kg of modified alumina powder prepared by carbonization, 24.0kg of metatitanic acid, and 1.5kg of hydroxycellulose were mixed and ball-milled to more than 200 mesh, and an appropriate amount of water and 4.0kg of phosphoric acid with a concentration of 52% were added and kneaded. squeeze into clover strips. Drying at 110-120° C. for 3 hours to obtain a carrier precursor. Based on the total amount of the carrier precursor as 100%, hydroxycellulose accounts for 1.5%, phosphoric acid accounts for 2.1%, and the rest is modified alumina powder and titanium-containing oxide prepared by carbonization.

[0029] Then the carrier precursor was calcined at 570° C. for 3 hours to obtain 90.5 kg of carrier. Among them, titanium-containing oxides (TiO 2 ) accounted for 21.7% of the total weight, and γ-alumina accounted for 78.3% of the total weight. The pore volume of the ca...

Embodiment 2

[0033] A hydrorefining catalyst is prepared through the following steps:

[0034] Preparation of the carrier: Mix 72.0kg of modified alumina powder prepared by carbonization, 24.0kg of metatitanic acid, and 4.0kg of scallop powder to a size above 200 mesh, add an appropriate amount of water and 8.0kg of phosphoric acid with a concentration of 52%, knead, squeeze into clover strips. Dry at 110-120° C. for 1 hour to obtain a carrier precursor. Based on 100% of the total weight of the carrier precursor, safflower powder accounts for 3.8%, phosphoric acid accounts for 4%, and the rest is modified alumina powder and titanium-containing oxide prepared by carbonization. .

[0035] The carrier precursor was calcined at 600°C for 3 h to obtain 91.5 kg of titanium-modified γ-alumina carrier, in which titanium oxide (TiO 2 ) accounted for 21.4% of the total weight, and γ-alumina accounted for 78.6% of the total weight. The pore volume of the carrier is 0.45mL / g, and the specific su...

Embodiment 3

[0039] A hydrorefining catalyst is prepared through the following steps:

[0040] Preparation of the carrier: Mix 72.0kg of modified alumina powder prepared by carbonization, 24.0kg of metatitanic acid, and 0.5kg of scallop powder to a size above 200 mesh, add an appropriate amount of water and 5.0kg of nitric acid with a concentration of 65%, knead, squeeze into clover strips. Drying at 110-120° C. for 3 hours to obtain a carrier precursor. Based on the total amount of the carrier precursor as 100%, the scallop powder accounts for 0.5%, nitric acid accounts for 3.3%, and the rest is modified alumina powder and titanium-containing oxide prepared by carbonization.

[0041] Then the carrier precursor was calcined at 570° C. for 3 hours to obtain 90.5 kg of carrier. Among them, titanium-containing oxides (TiO 2 ) accounted for 21.7% of the total weight, and γ-alumina accounted for 78.3% of the total weight. The pore volume of the carrier is 0.55mL / g, and the specific surfac...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
specific surface areaaaaaaaaaaa
specific surface areaaaaaaaaaaa
specific surface areaaaaaaaaaaa
Login to View More

Abstract

The invention discloses a hydrofining catalyst and a preparation method thereof, belonging to the field of catalysts used in the petroleum-chemical industry. The hydrofining catalyst disclosed herein comprises a carrier, an active component and an auxiliary agent, wherein the carrier is Ti-modified gamma-alumina, the active component comprises oxides of Mo, Co and Ni, and the auxiliary agent comprises oxides of rare earth. The catalyst is characterized in that: based on 100% of the total weight of the catalyst, Co (measured in CaO) in the active component accounts for 2.0-7.5% of the total weight of the catalyst, Mo (measured in MoO3) in the active component accounts for 4.0-18.0% of the total weight of the catalyst, Ni (measured in NiO) in the active component accounts for 0.2-5.0% of the total weight of the catalyst, the auxiliary agent accounts for 0.05-1.0% of the total weight of the catalyst, and the balance consists of the carrier. According to the invention, the catalyst prepared by the formula and the method disclosed in the invention can carry out hydrogenation on saturated monoolefine while the catalyst is used for carrying out hydrodesulfurization on oils, can be suitable for technical requirements of heavy oriention, changeable sulphur content, and high air speed of hydrogenation liquid for pyrolysis gasoline two-stage hydrogenated raw materials, and simultaneously, the catalyst has the advantages of low activation temperature and low loss of aromatics in the hydrogenation process.

Description

technical field [0001] A hydrorefining catalyst and a preparation method thereof belong to the field of petrochemical catalysts. Background technique [0002] During the steam cracking of hydrocarbons to produce olefins, the by-product C 5 above pyrolysis gasoline. Pyrolysis gasoline contains different degrees of unsaturated and easily oxidized hydrocarbons, such as diolefins and alkenyl aromatics. These compounds are prone to polymerization to form colloids, so that pyrolysis gasoline cannot be used directly. In industry, it is usually less than C in pyrolysis gasoline 5 , higher than C 9 After the fraction cut off, the middle distillate (C 6 ~C 8 ) is processed by a two-stage hydrogenation method. One-stage selective hydrogenation is mainly to remove diolefins, and then undergo two-stage hydrogenation to remove monoolefins and impurities such as S, N, and O, and then use them as raw materials for aromatics extraction. [0003] Since 1958, when UOP Corporation of th...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): B01J23/887C10G45/08
Inventor 王昊余汉涛姜建波种道文
Owner CHINA PETROLEUM & CHEM CORP
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Eureka Blog
Learn More
PatSnap group products