Embolic material composite and preparation method thereof
A material composition and embolization technology, applied in the field of materials, can solve problems such as mass effect and patient discomfort, and achieve the effects of preventing blood recanalization, accelerating vascular endothelialization, and reducing quality
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
preparation example Construction
[0032] The present invention also provides a preparation method of embolic material composition, comprising:
[0033] Adding polyethylene-vinyl alcohol to dimethyl sulfoxide to obtain a first solution;
[0034] adding a degradable polymer to the first solution to obtain a second solution;
[0035] A contrast agent is added to the second solution to obtain an embolic material composition.
[0036] The addition of the polyethylene-vinyl alcohol into the dimethyl sulfoxide is preferably carried out in an argon atmosphere, preferably by stirring to achieve the purpose of thorough mixing.
[0037] The adding of the degradable polymer to the first solution is preferably carried out in an argon atmosphere, preferably by stirring to achieve the purpose of thorough mixing.
[0038] According to the present invention, after the contrast agent is added to the second solution to obtain the embolic material composition, the embolic material composition is preferably put into a container,...
Embodiment 1
[0044] Add 10 g of EVOH with a number average molecular weight of 60,000 to 100 ml of DMSO, and stir for 2 hours at a temperature of 50° C. in an argon atmosphere to obtain a first solution;
[0045] Add 3 g of polylactic acid with a number average molecular weight of 150,000 to the first solution, and stir for 5 hours at a temperature of 70° C. in an argon atmosphere to obtain a second solution;
[0046] Add 30 g of tantalum powder to the second solution, stir until it is uniformly dispersed, put it into a container, seal it, sterilize it and store it.
Embodiment 2
[0048] Add 8 g of EVOH with a number average molecular weight of 65,000 to 100 ml of DMSO, and stir for 2 hours at a temperature of 50° C. in an argon atmosphere to obtain a first solution;
[0049] Add 3 g of gelatin with a number average molecular weight of 40,000 to the first solution, and stir for 3 hours at a temperature of 50° C. in an argon atmosphere to obtain a second solution;
[0050] Add 30 g of tantalum powder to the second solution, stir until it is uniformly dispersed, put it into a container, seal it, sterilize it and store it.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com