Embodiment 1
[0016] Embodiment 1: a kind of preparation method of color steel waterproof and thermal insulation coating The preparation method is as follows: (the material proportion mentioned below is by weight)
[0017] (1) Liquid material:
[0018] ① First put 10 parts of water into the mixer, add 0.5 parts of dispersible latex powder and stir and emulsify for 5 minutes.
[0019] ② Add 0.3 part of dibutyl phthalate, 0.2 part of polyacrylamide, 0.1 part of sodium alginate, 0.3 part of preservative, and 0.1 part of defoamer, and then stir and polymerize for 5 minutes.
[0020] ③ Then add 15 parts of vitrified microbeads, 5 parts of sepiolite, and 1 part of sericite, stir and polymerize for 3 minutes.
[0021] ④ Add 20 parts of BW-903 construction waterproof glue, stir and polymerize for 5 minutes and then fill the barrel.
[0022] (2) Powder:
[0023] Put 5 parts of aluminate cement, 15 parts of white Portland cement, and 0.2 parts of polypropylene fiber into the mixer and mix for 3 mi...
Embodiment 2
[0026] Embodiment 2: a kind of preparation method of color steel waterproof and thermal insulation coating The preparation method is as follows: (the material proportion mentioned below is by weight)
[0027] (1) Liquid material:
[0028] ① First put 12 parts of water into the mixer, add 0.6 parts of dispersible latex powder and stir and emulsify for 5 minutes.
[0029] ② Add 0.4 part of dibutyl phthalate, 0.3 part of polyacrylamide, 0.2 part of sodium alginate, 0.4 part of preservative, and 0.2 part of defoamer, and then stir and polymerize for 5 minutes.
[0030] ③Then add 17 parts of vitrified microbeads, 8 parts of sepiolite, and 2 parts of sericite, stir and polymerize for 3 minutes.
[0031] ④ Then add 21 parts of BW-903 construction waterproof glue, stir and polymerize for 5 minutes and then fill the barrel.
[0032] (2) Powder:
[0033] Put 7 parts of aluminate cement, 16 parts of white Portland cement, and 0.3 parts of polypropylene fiber into the mixer and mix for...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com