Method for producing metallic high temperature transfer base paper
A production method and technology for transferring base paper, which can be applied to paper, papermaking, papermaking machines, etc., can solve the problems of paper peeling difficulty, paper brittleness, coking and other problems, and achieve the effect of bright color, full pattern and resource saving.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] Embodiment 1, adopt 70% Canadian imported bleached softwood pulp and 30% Canadian imported bleached hardwood pulp, viscous beating through φ450 double disc mills after pulping, and then add chemical auxiliary materials with an amount of pulp weight percent:
[0024] Wet strength agent 1%
[0025] Aluminum Sulfate 3%
[0027] Stripper 0.1%
[0028] Retention aid 0.03%
[0029] After copying, the base paper is rewound by an upward-drawing rewinder, and its transfer effect is good.
[0030] Main technical indicators of finished paper:
[0031] 1. Tensile strength (MD): 1.2KN / m
[0032] 2. Tightness: 0.7g / cm 3
[0033] 3. Tear degree: 280mN
[0034] 4. Smoothness: (front) 500s; (reverse) 10s
[0035] 5. Sizing degree: 0.75mm;
[0036] 6. Gloss: 1.25mm
Embodiment 2
[0037] Embodiment 2, adopting 50% of Canadian imported bleached softwood pulp and 50% of Canadian imported bleached hardwood pulp, adding chemical auxiliary materials whose consumption is the percentage by weight of the slurry after pulping:
[0038] Wet strength agent 3%
[0039] High temperature resistant agent 3%
[0040] Starch 4%
[0041] Aluminum Sulfate 3%
[0043] Stripper 0.3%
[0044] Retention aid 0.05%
[0045] After copying, the base paper is rewound by an upward-drawing rewinder, and its transfer printing and peeling effect is good.
[0046] Main technical indicators of finished paper:
[0047] 1. Tensile strength (MD): 1.3KN / m
[0048] 2. Tightness: 0.72g / cm 3
[0049] 3. Tear degree: 270mN
[0050] 4. Smoothness: (front) 655s; (reverse) 10s
[0051] 5. Sizing degree: 1.25mm;
Embodiment 3
[0052] Embodiment 3, adopt 60% Canadian imported bleached softwood pulp and 40% Canadian imported bleached hardwood pulp, add the chemical auxiliary material that consumption is pulp weight percentage after pulping:
[0053] Wet strength agent 2%
[0054] High temperature resistant agent 3%
[0055] Starch 2%
[0056] Aluminum Sulfate 3%
[0058] Stripper 1%
[0059] Retention aid 0.05%
[0060] After copying, it is rewound by an upward rewinding machine to make base paper, and the printing and transfer peeling effect is good.
[0061] Main technical indicators of finished paper:
[0062] 1. Tensile strength (MD): 1.6KN / m
[0063] 2. Tightness: 0.75g / cm 3
[0064] 3. Tear degree: 320mN
[0065] 4. Smoothness: (front) 800s; (reverse) 10s
[0066] 5. Sizing degree: 1.0mm;
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com