A hardwood pulp and production process technology, applied in papermaking, paper machine, pulp bleaching, etc., can solve the problems of slow dissolution of hemicellulose, severe conditions, and difficulty in reducing polymerization, so as to reduce production costs, increase methylcellulose content, The effect of reducing pollution
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0043] Embodiment 1: sulfate method one
[0044] 1. Use 6000Kg of paper-making grade hardwood pulp board, and sort it by a pager.
[0045] 2. Soak it into a 3.5% (2.5-5.5) pulp porridge with 10% (8-14) NaOH.
[0046] 3. Use the porridge pump to send it into the press to squeeze and loosen the dispersed fibers.
[0047] 4. Put the pressed wood pulp into the digester for cooking. The process conditions are: (1) Cooking agent: NaOH+Na 2 S, the total alkali concentration of the cooking liquid is 80g / l (60-100), and the liquid ratio is 1:3.5 (3.0-4.0); (2) The initial temperature of the cooking liquid is ≥40°C; (3) Preheating for 10-15 minutes to 105 ±5°C; (4) Stop steam and then run dry for 25-30 minutes; (5) Adopt 2 times of small steam release and 3 times of heating curve, and the total heating time is 2 hours; (6) The holding temperature is 172±2°C. (145-172)
[0048] 5. Send the above-mentioned wood pulp slurry obtained by cooking from the dumping tank to the squeeze washing...
Embodiment 2
[0052] Embodiment 2: sulfate method two
[0053] 1. Use 6000Kg of paper-making grade hardwood pulp board, and sort it by a pager.
[0054] 2. Immerse into a slurry porridge with a concentration of 4.5% (2.5-5.5) with 8% (8-14) NaOH.
[0055] 3. Use the porridge pump to send it into the press to squeeze and loosen the dispersed fibers.
[0056] 4. Put the pressed wood pulp into the digester for cooking. The process conditions are: (1) Cooking agent: NaOH+Na 2 S, the total alkali concentration of the cooking liquid is 100g / l (60-100), and the liquid ratio is 1:3.5 (3.0-4.0); (2) The initial temperature of the cooking liquid is ≥40°C; (3) Preheating for 10-15 minutes to 105 ±5°C; (4) Stop steam and then run dry for 25-30 minutes; (5) Adopt 2 times of small steam release and 3 times of heating curve, the total heating time is 2 hours; (6) The holding temperature is 155±2°C. (145-172)
[0057] 5. Send the above-mentioned wood pulp slurry obtained by cooking from the dumping tan...
Embodiment 3
[0061] Embodiment 3: Sulfate method three
[0062] 1. Use 6000Kg of paper-making grade hardwood pulp board, and sort it by a pager.
[0063] 2. Dipping into a 4.5% (2.5-5.5) pulp porridge with 6% NaOH.
[0064] 3. Use the porridge pump to send it into the press to squeeze and loosen the dispersed fibers.
[0065] 4. Put the pressed wood pulp into the digester for cooking. The process conditions are: (1) Cooking agent: NaOH+Na 2 S, the total alkali concentration of the cooking liquid is 120g / l (60-100), and the liquid ratio is 1:3.5 (3.0-4.0); (2) The initial temperature of the cooking liquid is ≥40°C; (3) Preheating for 10-15 minutes to 105 ±5°C; (4) Stop steam and then run dry for 25-30 minutes; (5) Adopt 2 times of small steam release and 3 times of heating curve, and the total heating time is 2 hours; (6) The holding temperature is 135°C.
[0066] 5. Send the above-mentioned wood pulp slurry obtained by cooking from the dumping tank to the squeeze washing material to ext...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com