A technology for lithium-ion batteries and positive electrode materials, applied in the field of lithium-ion battery positive electrode materials using microwaves, can solve problems such as the inability to restore the structure of the recycled positive electrode materials, the inability to achieve complete recovery, and the structural defects of the positive electrode materials, so as to achieve effective recovery and suppression Li-nickel mixed row, the effect of reducing energy consumption
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0043] LiNi 0.56 Co 0.12 Mn 0.32 O 2 (N562 for short) The ternary positive electrode sheet is broken and sent to the NMP ultrasonic cell. After ultrasonication at 50 °C for 20 minutes, the current collector aluminum foil is filtered out with a 300-mesh screen, and then the ultrasonic cell solution is poured into the ceramic filter plate filter and collected. The positive black powder obtained by filtration. Wash with absolute ethanol and dry to obtain the recovered ternary positive electrode material after purification and impurity removal.
[0044] The purified ternary cathode material obtained above and the LiOH lithium source were mixed uniformly, the Li / TM was adjusted to 1.02, and the lithium supplementation was carried out directly under the condition of pure oxygen, the microwave frequency was 28GHz, and the microwave treatment time was 2h.
Embodiment 2
[0046] LiNi 0.56 Co 0.12 Mn 0.32 O 2 (N562 for short) The ternary positive electrode sheet is broken and sent to the NMP ultrasonic cell. After ultrasonication at 50 °C for 20 minutes, the current collector aluminum foil is filtered out with a 300-mesh screen, and then the ultrasonic cell solution is poured into the ceramic filter plate filter and collected. The positive black powder obtained by filtration. Then use high (3mol / L), medium (1mol / L) and low (0.2mol / L) NaOH lye solutions to wash and filter in stages to obtain ternary cathode black powder, and finally wash with absolute ethanol and After drying, the recovered ternary positive electrode material after purification and impurity removal is obtained.
[0047] The purified ternary cathode material obtained above and the LiOH lithium source were mixed uniformly, the Li / TM was adjusted to 1.02, and the lithium supplementation was carried out directly under the condition of pure oxygen, the microwave frequency was 28GH...
Embodiment 3
[0049] LiNi 0.56 Co 0.12 Mn 0.32 O 2 (N562 for short) The ternary cathode sheet is crushed and placed in a high-temperature box furnace, heat-treated at 500 °C for 5 hours, and the cathode black powder is obtained by vibrating screening. The ternary cathode black powder was washed with three concentrations of lye of high (3mol / L), medium (1mol / L) and low (0.2mol / L) in turn to wash the ternary cathode material, and finally washed and dried with absolute ethanol. , that is, the purified ternary cathode material is obtained.
[0050] The purified ternary cathode material was mixed with LiOH uniformly, the Li / TM ratio was adjusted to 1.02, the lithium was directly supplemented by microwave under oxygen-containing conditions, the microwave frequency was controlled to 28GHZ, and the microwave treatment time was 2h.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com