Calcined rounded colored sand
A calcining and rounding technology, which is applied to clay mixing devices, grinders, clay preparation devices, etc., can solve the problems of cracks in sand and gravel particles, erosion of decorative layers, sharp edges and corners, etc., to achieve long shelf life, uniform color, and increased use. The effect of longevity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] A kind of calcined round colored sand, its manufacturing process is as follows.
[0019] Step 1: The original sand is rounded, and the basalt is poured into the sander, and the edges and corners of the basalt are rounded to obtain rounded basalt;
[0020] Step 2: Mix raw materials, pour the rounded basalt obtained in Step 1 into a mixing tank, add kaolin and pigments and mix for 1 minute, then add binder and stir for 30 minutes to achieve full mixing;
[0021] Step 3: raw material drying, conveying the mixture obtained in step 2 to a kiln for drying for 20 minutes to obtain a dry material;
[0022] Step 4: Secondary mixing, transfer the dry material obtained in step 3 out of the kiln for packaging, then pour it back into the mixing tank, add glaze and binder to completely wrap the surface of each particle;
[0023] Step 5: preheating and calcining, conveying the secondary mixture obtained in step 4 into a kiln for preheating at 300°C, and calcining at 800°C to obtain a...
Embodiment 2
[0026] A kind of calcined round colored sand, its manufacturing process is as follows.
[0027] Step 1: The original sand is rounded, and the granite is poured into the sander, and the edges and corners of the granite are rounded to obtain rounded basalt;
[0028] Step 2: Mix raw materials, pour the rounded granite obtained in Step 1 into a mixing tank, add kaolin and pigments and mix for 1 minute, then add binder and stir for 30 minutes to achieve full mixing;
[0029] Step 3: raw material drying, conveying the mixture obtained in step 2 to a kiln for drying for 20 minutes to obtain a dry material;
[0030] Step 4: Secondary mixing, transfer the dry material obtained in step 3 out of the kiln for packaging, then pour it back into the mixing tank, add glaze and binder to completely wrap the surface of each particle;
[0031] Step 5: preheating and calcining, conveying the secondary mixture obtained in step 4 into a kiln for preheating at 290°C, and calcining at a temperature ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com