Preparation method of Bi-2212 superconducting thin film
A technology of bi-2212 and bi2212, applied in chemical instruments and methods, inorganic chemistry, bismuth compounds, etc., can solve the problems of high equipment cost and maintenance, high vacuum environment, poor film quality, etc. The effect of high efficiency and low cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] This embodiment includes the following steps:
[0027] Step 1. Mix Bi2212 powder with glacial acetic acid, and then heat and reflux under magnetic stirring conditions to obtain acetate solution; the mass ratio of Bi2212 powder and glacial acetic acid is 1:6, and the reflux temperature is 100°C , the time is 6h, the speed of the magnetic stirring is 300r / min;
[0028] Step 2, stirring after adding propionic acid to the acetate solution obtained in step 1, to obtain a film-making precursor solution; the volume of the propionic acid and acetate solution is 1:1;
[0029] Step 3, the film-making precursor solution obtained in step 2 is coated on the pure silver substrate by the dip coating method, and then dried and pre-decomposed successively to obtain a pre-decomposed Bi2212 thin film on the pure silver substrate; the pre-decomposed The temperature is 400°C, the heating rate is 40°C / h, and the holding time is 5h; the drying temperature is 85°C;
[0030] Step 4, the pre-d...
Embodiment 2
[0033] This embodiment includes the following steps:
[0034] Step 1. Mix Bi2212 powder with glacial acetic acid, then heat and reflux under magnetic stirring conditions to obtain acetate solution; the mass ratio of Bi2212 powder and glacial acetic acid is 1:9, and the reflux temperature is 120°C , the time is 3h, the speed of the magnetic stirring is 200r / min;
[0035] Step 2, add propionic acid to the acetate solution obtained in step 1 and stir to obtain a film-making precursor solution; the volume of the propionic acid and acetate solution is 1:2;
[0036]Step 3, the film-making precursor solution obtained in step 2 is coated on the pure silver substrate by the dip coating method, and then dried and pre-decomposed successively to obtain a pre-decomposed Bi2212 thin film on the pure silver substrate; the pre-decomposed The temperature is 500°C, the heating rate is 60°C / h, and the holding time is 3h; the drying temperature is 95°C; the process of coating, drying and pre-dec...
Embodiment 3
[0040] This embodiment includes the following steps:
[0041] Step 1. Mix Bi2212 powder with glacial acetic acid, and then heat and reflux under magnetic stirring conditions to obtain acetate solution; the mass ratio of Bi2212 powder and glacial acetic acid is 1:7.5, and the reflux temperature is 110°C , the time is 4h, and the speed of the magnetic stirring is 250r / min;
[0042] Step 2, add propionic acid to the acetate solution obtained in step 1 and stir to obtain a film-making precursor solution; the volume of the propionic acid and acetate solution is 1:1.5;
[0043] Step 3, the film-making precursor solution obtained in step 2 is coated on the pure silver substrate by the dip coating method, and then dried and pre-decomposed successively to obtain a pre-decomposed Bi2212 thin film on the pure silver substrate; the pre-decomposed The temperature is 450°C, the heating rate is 50°C / h, and the holding time is 4h; the drying temperature is 95°C; the process of coating, dryin...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com