Embodiment 1 and comparative example 1
[0040] The main agent A component is prepared according to the following weight parts:
[0041] component name Example 1 Comparative Example 1 DBTDL 0.08 0.68 MIBK 14.00 14.00 BAC 14.00 14.00 MEK 12.00 11.40 DBE 2.00 2.00 GALSTAFFMX-353 36.00 36.00 A86 5.00 5.00 BYK258 8.00 8.00 BYK399 0.50 0.50 BYK378 1.50 1.50 K-500 6.00 6.00 6900-20X 1.00 1.00
[0042] Curing agent B component is Desmodur N3390.
[0043] Prepare diluent C component according to the following weight parts:
[0044]
[0045]
[0046] Dilute the components A, B and C according to the ratio of 5:1:2.5. After the thinning, the viscosity of the coating-2 cups is 8 to 12s, then spray construction, and finally bake at 55 ℃ for 13 minutes. .
[0047] The test results of the paint film test of Example 1 and Comparative Example 1 are shown in the following table:
[0048]
[0049] It can be seen from the above t...
Embodiment 2~3
[0051] The main agent A component is prepared according to the following weight parts:
[0052] component name Example 2 Example 3 DABCOT12 0.05 0.10 MIBK 18.00 12.00 BAC 12.00 18.00 MEK 15.00 11.00 DBE 2.20 1.80 GALSTAFFMX-353 33.00 39.00 A86 6.00 4.00 BYK258 3.00 10.00 BYK399 0.70 0.30 BYK378 1.20 1.80 K-500 7.00 5.00 6900-20X 0.90 1.10
[0053] Curing agent B component is Desmodur N3390.
[0054] Prepare diluent C component according to the following weight parts:
[0055] component name Example 2 Example 3 EAC 45.00 53.00 DAA 34.00 31.00 IPA 11.00 7.00 DBTDL 1.50 1.00 PDO 10.50 7.00
[0056] In Example 2, component A, component B and component C were diluted at a ratio of 4:1:3, and the viscosity of the diluted coating-2 cups was 8 to 12s, and then spraying was carried out, and finally at 50 ℃ bake for 15min.
[0057] In E...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com