An inorganic fiber and thermal insulation board technology, applied in the field of thermal insulation materials, can solve the problems of high performance production cost, inability to continuous production, rapid strength decay, etc., achieve high hydrophobicity, improve density uniformity, and reduce fiber diameter.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0035] This embodiment provides an inorganic fiber insulation board, including the following raw material components in parts by mass:
[0036] 15 parts of metallurgical slag, 50 parts of coal gangue, 30 parts of washed Longyan soil, 45 parts of alumina, 30 parts of silicon oxide, 10 parts of talcum powder and 4 parts of fluorite.
[0037] The preparation method of above-mentioned inorganic fiber insulation board comprises the steps:
[0038] Step 1. Weigh each component according to the designed ratio, mix the weighed components evenly, heat to 1460°C and melt to obtain a liquid slurry;
[0039] Step 2, centrifuging the liquid slurry under the condition of 600r / min to spin into superfine fibers with an average diameter of 4.8 μm and collecting them to obtain fibers;
[0040] Step 3: Compact and shape the fiber into a flat plate with a pressure of 1.2 MPa, and then perform acupuncture with a density of 180 needles / m 2 , get fiber mat;
[0041] Step 4, the aluminum sol and s...
Embodiment 2
[0045] This embodiment provides an inorganic fiber insulation board, including the following raw material components in parts by mass:
[0046]20 parts of metallurgical slag, 35 parts of coal gangue, 10 parts of washed Longyan soil, 60 parts of alumina, 50 parts of silicon oxide, 8 parts of talcum powder and 5 parts of fluorite.
[0047] The preparation method of above-mentioned inorganic fiber insulation board comprises the steps:
[0048] Step 1. Weigh each component according to the designed ratio, mix the weighed components evenly, heat to 1430°C and melt to obtain a liquid slurry;
[0049] Step 2, centrifuge spinning the liquid slurry under the condition of 640r / min, spin it into superfine fibers with an average diameter of 4.0 μm and collect them to obtain fibers;
[0050] Step 3: Compact and shape the fiber into a flat plate with a pressure of 1.0 MPa, and then perform acupuncture with a density of 150 needles / m 2 , get fiber mat;
[0051] Step 4, the aluminum sol an...
Embodiment 3
[0055] This embodiment provides an inorganic fiber insulation board, including the following raw material components in parts by mass:
[0056] 30 parts of metallurgical slag, 20 parts of coal gangue, 20 parts of washed Longyan soil, 30 parts of alumina, 40 parts of silicon oxide, 5 parts of talcum powder and 3 parts of fluorite.
[0057] The preparation method of above-mentioned inorganic fiber insulation board comprises the steps:
[0058] Step 1. Weigh each component according to the designed ratio, mix the weighed components evenly, heat to 1445°C and melt to obtain a liquid slurry;
[0059] Step 2, centrifuge spinning the liquid slurry under the condition of 680r / min, spin it into superfine fibers with an average diameter of 3.5 μm and collect them to obtain fibers;
[0060] Step 3: Compact and shape the fiber into a flat plate with a pressure of 0.8 MPa, and then perform acupuncture with a density of 120 needles / m 2 , get fiber mat;
[0061] Step 4, the aluminum sol a...
PUM
Property | Measurement | Unit |
---|---|---|
diameter | aaaaa | aaaaa |
compressive strength | aaaaa | aaaaa |
compressive strength | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com