A treatment method and leaching solution technology are applied in the treatment field of cobalt intermediate products, which can solve the problems of large amount of chemical reagents, increased waste residue weight and high cost, and achieve the effects of improving iron removal, leaching effect and low price.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] A method for processing cobalt intermediates, characterized in that: comprising the steps of:
[0027] S1 Acid-dissolution leaching: add cobalt intermediate product into water, prepare ore slurry, add sulfuric acid leaching during stirring, wherein the composition of cobalt intermediate product is as follows: containing 26.90% of cobalt, containing 1.58% of copper, containing 3.99% of manganese, containing 1.62% of calcium, containing Manganese 4.09%, iron 5.09%;
[0028] S11: Take 200g of the cobalt intermediate product in a 3L beaker, add 1000mL of water, heat in a 60°C water bath, stir evenly and set aside;
[0029] S12: Adding mass concentration to the spare slurry is 1.84g / cm 3 Sulfuric acid to adjust pH=1.5, react for 30min;
[0030] S2 Reductive leaching: add hydrogen peroxide as a reducing agent for further leaching, and then filter to obtain leaching liquid and leaching residue;
[0031] S21: Slowly add 40ml of hydrogen peroxide to the S12 slurry, and contin...
Embodiment 2
[0036] A method for processing cobalt intermediates, characterized in that: comprising the steps of:
[0037] S1 Acid-dissolution leaching: add cobalt intermediate product into water, prepare ore slurry, add sulfuric acid leaching during stirring, wherein the composition of cobalt intermediate product is as follows: containing 26.90% of cobalt, containing 1.58% of copper, containing 3.99% of manganese, containing 1.62% of calcium, containing Manganese 4.09%, iron 5.09%;
[0038] S11: Take 200g of the cobalt intermediate product in a 3L beaker, add 1000mL of water, heat in a 60°C water bath, stir evenly and set aside;
[0039] S12: Adding mass concentration to the spare slurry is 1.84g / cm 3 Sulfuric acid to adjust pH=1.8, react for 30min;
[0040] S2 Reductive leaching: add hydrogen peroxide as a reducing agent for further leaching, and then filter to obtain leaching liquid and leaching residue;
[0041] S21: Slowly add 50 ml of hydrogen peroxide to the S12 slurry, and conti...
Embodiment 3
[0046] A method for processing cobalt intermediates, characterized in that: comprising the steps of:
[0047] S1 Acid-dissolution leaching: add cobalt intermediate product into water, prepare ore slurry, add sulfuric acid leaching during stirring, wherein the composition of cobalt intermediate product is as follows: containing 26.90% of cobalt, containing 1.58% of copper, containing 3.99% of manganese, containing 1.62% of calcium, containing Manganese 4.09%, iron 5.09%;
[0048] S11: Take 600g of the cobalt intermediate product in a 9L beaker, add 3000mL of water, heat in a 60°C water bath, stir evenly and set aside;
[0049] S12: Adding mass concentration to the spare slurry is 1.84g / cm 3 Sulfuric acid to adjust pH=1.5, react for 30min;
[0050] S2 Reductive leaching: add hydrogen peroxide as a reducing agent for further leaching, and then filter to obtain leaching liquid and leaching residue;
[0051]S21: Slowly add 120ml of hydrogen peroxide to the S12 slurry, and contin...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com