A double degradation, plastic bag technology, applied in the field of plastic films, can solve the problems of poor oxidation resistance, short service life and general degradation effect of photobiodegradable plastics, and achieve the goal of improving degradable performance, improving comprehensive performance and accelerating degradation speed. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] Weigh the raw materials in the following weight ratio: 20 parts of polyethylene, 20 parts of calcium carbonate, 15 parts of microcrystalline starch, 10 parts of xyloglucan, 10 parts of chitin, 2 parts of diphenylcyclopropenone, disulfurized carbamic acid 1 part of iron, 1 part of titanate coupling agent, 1 part of nano titanium dioxide, 1 part of simethicone, 2 parts of sorbitol, 2 parts of phthalic acid, 2 parts of sodium carboxymethyl cellulose, oxidized polyethylene 2 parts wax, 2 parts mannitol stearate, 2 parts acetic acid. Prepare as follows:
[0023] (1) Grind calcium carbonate to a particle size of 700 mesh, put it in an oven at a temperature of 100°C, and dry it until the water content is 2%, add it to a high-speed stirring mixer with a titanate coupling agent, and mix for 5 minutes ;
[0024] (2) Add polyethylene, microcrystalline starch, diphenylcyclopropenone, iron disulfide carbamate, and nano-titanium dioxide to the high-speed mixer and mix for 5 minutes...
Embodiment 2
[0030] Weigh the raw materials in the following weight proportions: 25 parts of polyethylene, 25 parts of calcium carbonate, 20 parts of microcrystalline starch, 15 parts of xyloglucan, 15 parts of chitin, 4 parts of diphenylcyclopropenone, disulfurized carbamic acid 3 parts of iron, 3 parts of titanate coupling agent, 2 parts of nano-titanium dioxide, 2 parts of simethicone, 3 parts of sorbitol, 3 parts of phthalic acid, 4 parts of sodium carboxymethyl cellulose, oxidized polyethylene 5 parts of wax, 5 parts of mannitol stearate, 5 parts of acetic acid.
[0031] Prepare as follows:
[0032] (1) Grind calcium carbonate to a particle size of 1000 mesh, put it in an oven at a temperature of 100°C, and dry it until the water content is 1.5%, add it to a high-speed mixer with a titanate coupling agent, and mix for 15 minutes;
[0033] (2) Add polyethylene, microcrystalline starch, diphenylcyclopropenone, iron disulfide carbamate, and nano-titanium dioxide to the high-speed mixer ...
Embodiment 3
[0039] Weigh the raw materials in the following weight proportions: 30 parts of polyethylene, 30 parts of calcium carbonate, 30 parts of microcrystalline starch, 20 parts of xyloglucan, 20 parts of chitin, 6 parts of diphenylcyclopropenone, disulfurized carbamic acid 5 parts of iron, 5 parts of titanate coupling agent, 3 parts of nano-titanium dioxide, 3 parts of simethicone, 5 parts of sorbitol, 4 parts of phthalic acid, 6 parts of sodium carboxymethyl cellulose, oxidized polyethylene 8 parts of wax, 8 parts of mannitol stearate, 8 parts of acetic acid.
[0040] Prepare as follows:
[0041] (1) Grind calcium carbonate to a particle size of 1200 mesh, put it in an oven at a temperature of 100°C, and dry it until the water content is 1%, add it to a high-speed stirring mixer with a titanate coupling agent, and mix for 20 minutes ;
[0042] (2) Add polyethylene, microcrystalline starch, diphenylcyclopropenone, iron disulfide carbamate, and nano-titanium dioxide to the high-speed...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com