Silane treating agent and preparation method thereof
The technology of a silane treatment agent and a silane coupling agent is applied in the direction of metal material coating process, etc., which can solve problems such as poor anti-corrosion performance, and achieve the effects of stable performance, dense and uniform polarization current density, and simple preparation.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0036] A silane treatment agent, each component of its composition raw material is composed as follows according to parts by weight:
[0037] KH560 2 copies;
[0038] Phytic acid 2 parts;
[0039] 8 parts of sodium nitrate;
[0040] Sodium molybdate 4 parts;
[0041] 70 parts of deionized water;
[0042] Formic acid was also included to adjust the pH of the solution to 4-5.
[0043] A preparation method of silane treatment agent, comprising the following steps:
[0044] Step 1: Add 2 parts of KH560 to 70 parts of deionized water and hydrolyze for 3 hours;
[0045] Step 2: Add 2 parts of phytic acid, 8 parts of sodium nitrate, and 3 parts of sodium molybdate in sequence and keep stirring for 20 minutes;
[0046] Step 3: When using a pH detector to monitor the pH value of the mixed solution in step 3 in real time, continuously add formic acid to the mixed solution in step 2 until the pH value of the mixed solution is adjusted to 4.0-5.0.
Embodiment 2
[0048] A silane treatment agent, each component of its composition raw material is composed as follows according to parts by weight:
[0049] KH560 3 copies;
[0050] 3 parts of phytic acid;
[0051] 10 parts of sodium nitrate;
[0052] 5 parts of sodium molybdate;
[0053] 80 parts of deionized water;
[0054] Formic acid was also included to adjust the pH of the solution to 4-5.
[0055] A preparation method of silane treatment agent, comprising the following steps:
[0056] Step 1: Add 3 parts of KH560 to 80 parts of deionized water and hydrolyze for 3 hours;
[0057] Step 2: Add 3 parts of phytic acid, 10 parts of sodium nitrate, and 5 parts of sodium molybdate in sequence and keep stirring for 20 minutes;
[0058] Step 3: When using a pH detector to monitor the pH value of the mixed solution in step 3 in real time, continuously add formic acid to the mixed solution in step 2 until the pH value of the mixed solution is adjusted to 4.0-5.0.
Embodiment 3
[0060] A silane treatment agent, each component of its composition raw material is composed as follows according to parts by weight:
[0061] KH560 4 copies;
[0062] Phytic acid 4 parts;
[0063] 12 parts of sodium nitrate;
[0064] Sodium molybdate 6 parts;
[0065] 90 parts of deionized water;
[0066] Formic acid was also included to adjust the pH of the solution to 4-5.
[0067] A preparation method of silane treatment agent, comprising the following steps:
[0068] Step 1: Add 4 parts of KH560 to 90 parts of deionized water and hydrolyze for 3 hours;
[0069] Step 2: Add 4 parts of phytic acid, 12 parts of sodium nitrate and 6 parts of sodium molybdate in sequence and keep stirring for 20 minutes;
[0070] Step 3: When using a pH detector to monitor the pH value of the mixed solution in step 3 in real time, continuously add formic acid to the mixed solution in step 2 until the pH value of the mixed solution is adjusted to 4.0-5.0.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com