[0013] 1. Add 23.5kg of deionized water to 12kg of water-based polyurethane and stir evenly;
[0014] 2. Add 6kg of deionized water to 3kg of epoxy acrylate UV resin and stir evenly;
[0015] 3. Add 2kg of deionized water to 0.7kg of dodecyl alcohol ester and stir evenly;
[0016] 4. Add 2 kg of deionized water to 0.4 kg of polyethylene terephthalate, and stir evenly;
[0017] 5. Add 1.5 kg of deionized water to 0.2 kg of bis(acetylacetone) ethoxy isopropoxy titanate, and stir evenly;
[0018] 6. Add 0.5 deionized water to 0.07kg sodium dodecyl diphenyl ether disulfonate, and stir evenly;
[0019] 7. Add 1 kg of deionized water to 0.6 kg of diglycidyl ether, and stir evenly;
[0020] 8. Mix the solutions obtained in the above steps, and add 46.03kg of ionized water and 0.3kg of nano-magnesium oxide, and stir for 4-6 hours;
[0021] 9. Add 0.2 kg of glacial acetic acid to the stirred solution in step 8, and stir for 1-2 hours.
Embodiment 2
[0023] 1. Add 24kg of deionized water to 11kg of water-based polyurethane and stir evenly;
[0024] 2. Add 8kg of deionized water to 4kg of epoxy acrylate UV resin and stir evenly;
[0025] 3. Add 2.5kg of deionized water to 0.8kg of dodecyl alcohol ester and stir evenly;
[0026] 4. Add 3 kg of deionized water to 0.6 kg of polyethylene terephthalate, and stir evenly;
[0027] 5. Add 1 kg of deionized water to 0.3 kg of bis(acetylacetone) ethoxy isopropoxy titanate, and stir evenly;
[0028] 6. Add 1 kg of deionized water to 0.09 kg of sodium dodecyl diphenyl ether disulfonate, and stir evenly;
[0029] 7. Add 2 kg of deionized water to 0.5 kg of diglycidyl ether, and stir evenly;
[0030] 8. Mix the solutions obtained in the above steps, and add 40.61 kg of ionized water and 0.4 kg of nano-magnesium oxide, and stir for 4-6 hours;
[0031] 9. Add 0.2 kg of glacial acetic acid to the stirred solution in step 8, and stir for 1-2 hours.
Embodiment 3
[0033] Water-based polyurethane 13%, epoxy acrylate UV resin 5%, lauryl alcohol ester 0.6%, polyethylene terephthalate 0.3%, bis(acetylacetone) ethoxy isopropoxy titanate 0.1%, sodium dodecyl diphenyl ether disulfonate 0.11%, neopentyl glycol diglycidyl ether 0.4%, nano-magnesium oxide 0.5%, glacial acetic acid 0.3%, and the balance is deionized water.
[0034] 1. Add 25kg of deionized water to 13kg of water-based polyurethane and stir evenly;
[0035] 2. Add 10kg of deionized water to 5kg of epoxy acrylate UV resin and stir evenly;
[0036] 3. Add 1.2kg of deionized water to 0.6kg of dodecyl alcohol ester and stir evenly;
[0037] 4. Add 1.8kg of deionized water to 0.3kg of polyethylene terephthalate, and stir evenly;
[0038] 5. Add 1 kg of deionized water to 0.1 kg of bis(acetylacetone) ethoxy isopropoxy titanate, and stir evenly;
[0039] 6. Add 1 kg of deionized water to 0.11 kg of sodium dodecyl diphenyl ether disulfonate, and stir evenly;
[0040] 7. Add 1 kg of dei...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com