A method for eliminating mottled defects on the surface of hot-rolled steel plates
A hot-rolled steel sheet and mottled technology, used in workpiece surface treatment equipment, metal rolling, metal rolling, etc., can solve the problem of controlling the structure and thickness of the iron oxide scale on the surface of the steel sheet. It does not involve how to eliminate the surface defects of the steel sheet, etc. problems, to ensure the surface quality and mechanical properties, eliminate chromatic aberration defects, and improve production efficiency.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0027] (1) Heat the slab to 1200°C, then descale with high-pressure water, the descaling temperature is 1150°C, and the water pressure is 16MPa during descaling;
[0028] (2) rough rolling the descaled steel plate, the temperature of rough rolling is 1100℃;
[0029] (3) The rough-rolled steel plate is subjected to finish rolling, the finish rolling temperature is 950°C, and the roller table speed is 1.4m / s;
[0030] (4) After finishing rolling, laminar flow cooling is used for water cooling, and segmental cooling is adopted, the water ratio is 2.3; the cooling water volume is 150m³ / h; the temperature of the steel plate after cooling is 680°C;
[0031] (5) The water-cooled steel plate is cooled in the air on the cooling bed.
[0032] After the steel plate is rolled and water-cooled, the photo of cooling on the cooling bed is as follows figure 1 shown. From figure 1 It can be seen that after the steel plate is hot-rolled, there is no cracking phenomenon of iron oxide scale o...
Embodiment 2
[0034] (1) Heat the slab to 1220°C, then descale with high-pressure water, the descaling temperature is 1180°C, and the water pressure is at least 17MPa during descaling;
[0035] (2) rough rolling the descaled steel plate, the temperature of rough rolling is 1120°C;
[0036] (3) The rough-rolled steel plate is subjected to finish rolling, the finish rolling temperature is 960°C, and the roller table speed is 1.5m / s;
[0037] (4) After finishing rolling, laminar flow cooling is used for water cooling, and segmental cooling is adopted, the water ratio is 2.4; the cooling water volume is 200m³ / h; the temperature of the steel plate after cooling is 700°C;
[0038] (5) The water-cooled steel plate is cooled in the air on the cooling bed.
[0039] After the steel plate is rolled and water-cooled, the photo of cooling on the cooling bed is as follows image 3 shown. From image 3 It can be seen that when the steel plate is cooled on the cooling bed, the surface is smooth and the...
Embodiment 3
[0041] (1) Heat the slab to 1240°C, then descale with high-pressure water, the descaling temperature is 1200°C, and the water pressure is 19MPa during descaling;
[0042] (2) rough rolling the descaled steel plate, the temperature of rough rolling is 1180°C;
[0043] (3) The rough-rolled steel plate is subjected to finish rolling, the final rolling temperature of the finish rolling is 980°C, and the roller table speed is 1.7m / s;
[0044] (4) After finishing rolling, laminar flow cooling is used for water cooling, and segmental cooling is adopted, the water ratio is 2.5; the cooling water volume is 250m³ / h; the temperature of the steel plate after cooling is 730°C;
[0045] (5) The water-cooled steel plate is cooled in the air on the cooling bed.
[0046] After the steel plate is rolled and water-cooled, the photo of cooling on the cooling bed is as follows Figure 5 shown. From Figure 5It can be seen that under the process conditions of Example 3, the surface of the steel...
PUM
Property | Measurement | Unit |
---|---|---|
thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com