Adhesive with anti-line-explosion function for corrugated paperboard production and preparation method of adhesive
A technology of corrugated cardboard and explosion-proof line, which is applied in the types of adhesives, starch adhesives, polymer adhesive additives, etc. Achieve the effect of improving cardboard consistency, increasing production costs and improving stability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0017] The preparation method of the adhesive with explosion-proof line function for the production of corrugated cardboard of this embodiment comprises the following steps:
[0018] Step 1: Add 200 kg of water into the cooked pulp tank, stir and slowly add 20 kg of cornstarch and 5 kg of sodium hydroxide in sequence, and stir for 12 minutes until the slurry is beige and transparent, and the cooked pulp is obtained;
[0019] Step 2: Add 800kg of water into the raw slurry tank, stir and slowly add 270kg of cornstarch, 2kg of borax in turn, stir for 5 minutes, then add 7kg of stabilizer, 2kg of enhancer, 1kg of sodium chloride in turn, and stir for 3 minutes;
[0020] Step 3: slowly pour the cooked pulp prepared in step 1 into the raw pulp tank in step 2, and stir for 20 minutes to obtain the adhesive with the function of explosion-proof wire.
Embodiment 2
[0022] The preparation method of the adhesive with explosion-proof line function for the production of corrugated cardboard of this embodiment comprises the following steps:
[0023] Step 1: Add 200 kg of water into the cooked pulp tank, stir and slowly add 25 kg of cornstarch and 7.5 kg of sodium hydroxide in sequence, and stir for 15 minutes until the slurry is beige and transparent, and the cooked pulp is obtained;
[0024] Step 2: Add 800kg of water into the raw slurry tank, stir and slowly add 350kg of cornstarch, 3kg of borax in turn, stir for 5 minutes, then add 9kg of stabilizer, 3kg of enhancer, 2kg of sodium chloride in turn, and stir for 3 minutes;
[0025] Step 3: slowly pour the cooked pulp prepared in step 1 into the raw pulp tank in step 2, and stir for 20 minutes to obtain the adhesive with the function of explosion-proof wire.
Embodiment 3
[0027] The preparation method of the adhesive with explosion-proof line function for the production of corrugated cardboard of this embodiment comprises the following steps:
[0028] Step 1: Add 200 kg of water into the cooked pulp tank, stir and slowly add 30 kg of cornstarch and 10 kg of sodium hydroxide in sequence, and stir for 18 minutes until the slurry is beige and transparent, and the cooked pulp is obtained;
[0029] Step 2: Add 800kg of water into the raw slurry tank, stir and slowly add 380kg of cornstarch, 4kg of borax in turn, stir for 5 minutes, then add 8kg of stabilizer, 2.5kg of enhancer, 3kg of sodium chloride in turn, and stir for 3 minutes;
[0030] Step 3: slowly pour the cooked pulp prepared in step 1 into the raw pulp tank in step 2, and stir for 20 minutes to obtain the adhesive with the function of explosion-proof wire.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com