A high-strength, stainless steel technology, applied in the field of atmospheric pressure remelting smelting high-nitrogen stainless steel, remelting high-strength stainless steel, can solve the problems of reducing the recycling value of waste materials, reducing the nitrogen content of high-nitrogen steel, waste of waste materials, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] Take 3700kg of high-nitrogen steel waste materials; prepare about 1300kg of high-nitrogen steel new materials, including 610kg of industrial pure iron, 160kg of ferrochrome nitride, 110kg of high-nitrogen ferrochrome, 160kg of micro-carbon ferrochrome, 240kg of electrolytic manganese metal, and 20kg of manganese nitride .
[0025] Specific smelting steps:
[0026] 1) Add all industrial pure iron and micro-carbon ferrochrome to the intermediate frequency induction furnace, add all electrolytic manganese metal after melting, and adjust the melt temperature to 1450°C;
[0027] 2) Gradually add high-nitrogen steel waste into the furnace to keep the melt temperature at 1450°C until it is completely melted into a melt;
[0028] 3) Gradually add high-nitrogen ferrochrome to the furnace at a rate of 100kg / min and keep the melt temperature at 1450°C;
[0029] 4) Gradually add ferrochromium nitride into the furnace at a rate of 100kg / min, and keep the melt temperature at 1450°C...
Embodiment 2
[0034] Take 1000kg of high-nitrogen steel waste materials; prepare about 4000kg of high-nitrogen steel new materials, including 1870kg of industrial pure iron, 1330kg of ferrochrome nitride, 650kg of electrolytic manganese metal, and 150kg of manganese nitride.
[0035] Melting steps:
[0036] 1) Add all industrial pure iron to the intermediate frequency induction furnace, add all electrolytic manganese metal after melting, and adjust the melt temperature to 1500°C;
[0037] 2) Gradually add high-nitrogen steel waste into the furnace to keep the melt temperature at 1500°C until it is completely melted into a melt;
[0038] 3) Gradually add ferrochromium nitride into the furnace at a rate of 300kg / min, and keep the melt temperature at 1500°C;
[0039] 4) Gradually add manganese nitride into the furnace at a rate of 100kg / min and keep the melt temperature at 1500°C;
[0040] 5) After all the nitrogen-containing alloys are added, keep the melt temperature at 1500°C, and at the ...
Embodiment 3
[0044] Take 2500kg of high-nitrogen steel waste materials; prepare about 2500kg of high-nitrogen steel new materials, including 610kg of industrial pure iron, 490kg of ferrochrome nitride, 160kg of high-nitrogen ferrochrome, 140kg of micro-carbon ferrochrome, and 500kg of electrolytic manganese metal.
[0045] Melting steps:
[0046] 1) Add all industrial pure iron and micro-carbon ferrochrome to the intermediate frequency induction furnace, add all electrolytic manganese metal after melting, and adjust the melt temperature to be between 1480°C;
[0047] 2) Gradually add high-nitrogen steel waste into the furnace to keep the melt temperature between 1550°C until it is completely melted into a melt;
[0048]3) Gradually add high-nitrogen ferrochromium into the furnace at a rate of 100kg / min and keep the melt temperature at 1550°C;
[0049] 4) Gradually add ferrochromium nitride into the furnace at a rate of 200kg / min, and keep the melt temperature at 1550°C;
[0050] 5) After...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com