Two-sided offset paper for paper bags and preparation method of two-sided offset paper
A technology of double-adhesive paper and internal sizing, applied in the field of papermaking, can solve problems such as poor printing effect, and achieve the effects of reducing paper traction, improving printing performance, and reducing pressure light.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0036] Paper basis weight is 50gsm
[0037] 1. Pulping
[0038] 100% bleached chemical pulp is used, the amount of hardwood bleached chemical pulp accounts for 70%, the amount of softwood bleached chemical pulp accounts for 20%, the high yield pulp accounts for 10%, and the Shore beating degree is 30°SR. Slurry (1 ton) was prepared after loose pulp, pulp cleaning, pulp refining or flaking, adding fiber modifying enzyme, 30ppm to pulp, and 45min treatment time.
[0039] 2. Add chemicals
[0040] Add alkyl ketene dimer (AKD) to the wet end, the consumption is 10 kg / ton of paper, alkenyl succinic anhydride (ASA) 0.5 kg / ton of paper, 150 kg / ton of filler, in this embodiment, the filler is precipitated carbonic acid Calcium or ground calcium carbonate, appropriate amount of starch enhancer. The appropriate amount here can be understood by those skilled in the art. 3. Surface sizing
[0041] Surface sizing starch coating amount 5g / m 2 .
[0042] 4. Post calendering
[0043] ...
Embodiment 2
[0046] Paper basis weight is 80gsm
[0047] 1. Pulping
[0048]100% bleached chemical pulp is used, the amount of hardwood bleached chemical pulp accounts for 75%, the amount of softwood bleached chemical pulp accounts for 15%, the high yield pulp accounts for 10%, and the Shore beating degree is 28°SR. Slurry (1 ton) is obtained after loose pulp, pulp cleaning, pulp refining or deflaking, adding fiber-modifying enzymes, and pulping at 40ppm for 30 minutes.
[0049] 2. Add chemicals
[0050] Add alkyl ketene dimer (AKD) to the wet end, the dosage is 9 kg / ton of paper, alkenyl succinic anhydride (ASA) 0.5 kg / ton of paper, 170 kg / ton of filler talcum powder.
[0051] 3. Surface sizing
[0052] Surface sizing starch coating amount 8g / m 2 .
[0053] 4. Post calendering
[0054] The pressure is controlled at 25kg / cm 2 .
[0055] The properties of the offset paper obtained in this example: the folding resistance is more than 200 times.
Embodiment 3
[0057] Paper base weight is 100gsm
[0058] 1. Pulping
[0059] 100% bleached chemical pulp is used, the amount of hardwood bleached chemical pulp accounts for 80%, the amount of softwood bleached chemical pulp accounts for 15%, and the high-yield pulp accounts for 5%. After loose pulp, pulp cleaning, pulp refining or deflaking, biological enzymes are added. , 80ppm to slurry, treatment time 60min, prepared slurry (1 ton).
[0060] 2. Add chemicals
[0061] Add alkyl ketene dimer (AKD) to the wet end, the dosage is 10 kg / ton of paper, alkenyl succinic anhydride (ASA) 0.8 kg / ton of paper, filler china clay 200 kg / ton of paper.
[0062] 3. Surface sizing
[0063] Surface sizing starch coating amount 10g / m 2 .
[0064] 4. Post calendering
[0065] The pressure is controlled at 30kg / cm 2 .
[0066] The performance of the offset paper obtained in this embodiment: the folding resistance is more than 150 times.
PUM
Property | Measurement | Unit |
---|---|---|
Base weigh | aaaaa | aaaaa |
Bulk | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com