Fully flushable biodegradable nonwoven wet wipes and method for producing the same
A non-woven fabric, biodegradable technology, applied in non-woven fabrics, textiles and papermaking, fiber treatment, etc., can solve the problem of waste of non-woven fabric wet wipes
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0037] Raw materials: 82% (weight ratio) of wood pulp fluff pulp, 18% (weight ratio) of 919 glue.
[0038] Non-woven production: After air-laid to form a fiber web, the weight of the fiber web is 45GSM, dilute the 919 glue by one time, spray on one side of the fiber web, then dry, and then spray the other side, control the amount of spraying, so that the non-woven fabric Weight at 55GSM.
[0039] Liquid wipes
[0040] 1. Normal dosing 1.5 parts of EDTA
[0041] Lecithin 0.8 parts
[0042] Aloe Vera Extract 10 parts
[0043] 3 parts glycerin
[0044] 1 part lanolin
[0045] 1.2 parts of citric acid
[0046] Add 80.5 parts of deionized pure water
[0047] 2. Passivation:
[0048] boric acid 2 parts
[0049] Cut the non-woven fabric into 150*200mm slices, fold them in a Z shape first, and then fold them in half. Folded 50 pieces of non-woven fabrics were folded neatly. Soak it in the wet wipe solution, put it into a plastic bag of appropriate size, and heat seal it. ...
Embodiment 2
[0051] Raw materials: 78% (weight ratio) of viscose fiber, 22% (weight ratio) of SKJ glue.
[0052] Non-woven production: After combing into a web to form a fiber web, the weight of the fiber web is 24GSM, dilute the SKJ glue twice, spray on one side of the fiber web, then dry, and then spray the other side, control the amount of spraying, so that the non-woven fabric Weight at 28GSM.
[0053] Liquid wipes:
[0054] 1. Normal dosing 1.5 parts of EDTA
[0055] Lecithin 0.8 parts
[0056] 3 parts glycerin
[0057] 1 part lanolin
[0058] 2 parts citric acid
[0059] Add 85.7 parts of deionized pure water
[0060] 2. Passivation: 6 parts of table salt
[0061] Cut the non-woven fabric into 150*200mm slices, fold them in a Z shape first, and then fold them in half. Soak the folded piece of non-woven fabric in the solution, put it into a plastic bag of appropriate size, and heat seal it.
Embodiment 3
[0063] Raw materials: 92% (weight ratio) of PLA biodegradable polymer, 8% (weight ratio) of SKJ type glue.
[0064] Non-woven production: In the spunbond method, after the polymer is spun, it is air-laid to form a fiber web. The weight of the fiber web is 20GSM. Dilute the SKJ type glue by one time, spray on one side of the fiber web, then dry, and then spray On the other hand, control the amount of spraying so that the weight of the nonwoven fabric is 22.5GSM.
[0065] Liquid wipes:
[0066] 1. Normal dosing 1.5 parts of EDTA
[0067] Lecithin 0.8 parts
[0068] 3 parts glycerin
[0069] 1 part lanolin
[0070] 2 parts citric acid
[0071] Add 90.7 parts of deionized pure water
[0072] 2. Passivation: Calcium chloride 1 part
[0073] Cut the non-woven fabric into 150*200mm slices, fold them in a Z shape first, and then fold them in half. Soak the folded nonwoven fabric in a stack of 30 pieces in the solution, put it into a plastic bag of appropriate size, and heat se...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com