A technology for knitting yarn and linen, which is applied to the production field of flax blended knitting yarn, can solve the problems of easy wrinkling of fabrics, difficulty in improving product quality, and greater restrictions on spinning fineness, and achieves clear and plump appearance and low cost. , the effect of less hairiness in the yarn
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0027] Embodiment 1: spinning the blended yarn of 24tex
[0028] (1) Mixing of raw materials
[0029] The blend ratio of linen / modal is 70 / 30; by weight blending method,
[0030] (2) Pre-spinning process:
[0031] ① Open and clean cotton
[0032] The lap weight is 383g / m,
[0033] ② Carding
[0034] Raw sliver weight is 19.5g / 5 m,
[0035] ③Drawing
[0036] Quantitative weight of first half-cooked strips: 17.1g / 5m, second-half-cooked strips quantitative: 16.2g / 5m, three-way (cooked strips) quantitative 14.7 g / 5m,
[0037] (3) Rotor spinning process
[0038] Temperature 25℃, relative humidity 75%
[0039] ① Opening roller speed: 7200r / min,
[0040] ②Diameter and speed of rotor
[0041] Rotor diameter: 52mm, rotor speed: 45000r / min,
[0042] ③ Twist factor: 370,
[0043] ④ Selection of other process parameters
[0044] The yarn drawing speed is 58.5m / min, and the tension draft is 0.98.
Embodiment 2
[0045] Embodiment 2: spinning the blended yarn of 28tex
[0046] (1) Mixing of raw materials
[0047] The blend ratio of linen / modal is 70 / 30; by weight blending method,
[0048] (2) Pre-spinning process:
[0049] ① Open and clean cotton
[0050] Lap basis weight is 401g / m,
[0051] ② Carding
[0052] The raw sliver weight is 21.3g / 5 m,
[0053] ③Drawing
[0054] Quantitative quantity of first half-cooked strips: 18.4g / 5m, quantitative quantity of double-semi-cooked strips: 17.6g / 5m, quantitative quantity of three-cured strips (cooked strips) 15.4 g / 5m,
[0055] (3) Rotor spinning process
[0056] Temperature 25℃, relative humidity 75%
[0057] ① Opening roller speed: 7600r / min,
[0058] ②Diameter and speed of rotor
[0059] Rotor diameter: 52mm, rotor speed: 48000r / min,
[0060] ③ Twist factor: 370,
[0061] ④ Selection of other process parameters
[0062] The yarn drawing speed is 58.5m / min, and the tension draft is 0.98.
Embodiment 3
[0063] Embodiment 3: spinning the blended yarn of 24tex
[0064] (1) Mixing of raw materials
[0065] The blend ratio of linen / modal is 60 / 40; by weight blending method,
[0066] (2) Pre-spinning process:
[0067] ① Open and clean cotton
[0068] The lap weight is 390g / m,
[0069] ② Carding
[0070] The raw sliver weight is 20.6g / 5 m,
[0071] ③Drawing
[0072] Quantitative weight of first half-cooked strips: 17.9g / 5m, second-half-cooked strips quantitative: 16.8g / 5m, triple (cooked strips) quantitative 15.1g / 5m,
[0073] (3) Rotor spinning process
[0074] Temperature 25℃, relative humidity 75%
[0075] ① Opening roller speed: 7200r / min,
[0076] ②Diameter and speed of rotor
[0077] Rotor diameter: 52mm, rotor speed: 45000r / min,
[0078] ③ Twist factor: 375,
[0079] ④ Selection of other process parameters
[0080] The yarn drawing speed is 58.5m / min, and the tension draft is 0.98.
PUM
Property | Measurement | Unit |
---|---|---|
twist factor | aaaaa | aaaaa |
twist factor | aaaaa | aaaaa |
twist factor | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com