Elastic peelable glue and method for carrying out local electroplating protection by using same
A local electroplating and stripping technology, applied in the field of electroplating, can solve the problems of mutual pollution of solutions, long production cycle, and endangering the health of operators, and achieve the effects of reducing production costs, improving production efficiency, and easy process control
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] Embodiment 1: a kind of elastic peelable glue, its formula is: styrene-butadiene-styrene copolymer (SBS) 30 weight parts, linear alkane base mineral oil 38 weight parts, C5 petroleum resin 30 weight parts , 2 parts by weight of antioxidant; wherein the antioxidant is tetrakis [methyl-β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester.
[0025] According to the above formula, put each component into a kneader with heating, melt and stir to uniformly discharge, granulate or flake to obtain the elastic peelable rubber.
[0026] The method for carrying out local electroplating protection with the elastic peelable adhesive in this embodiment is as follows:
[0027] (1) Put the elastic peelable glue into a temperature-controllable container, then heat it, and keep the temperature at 140-180°C. After the elastic peelable glue is completely melted, let it stand for 10-20 minutes to start using;
[0028] (2) Immerse the workpiece to be electroplated in the ...
Embodiment 2
[0032] Embodiment 2: substantially the same as Example 1, the difference is 35 parts by weight of styrene-ethylene-hydrogenated butadiene-styrene copolymer (SEBS), 40 parts by weight of naphthenic mineral oil, 25 parts by weight of terpene resin share.
[0033] In the method of using the elastic peelable adhesive in this embodiment for partial electroplating protection, the workpiece after dipping is immersed in cold water for 10 minutes to cool.
Embodiment 3
[0034] Embodiment 3: basically the same as Embodiment 1, the difference is 40 parts by weight of styrene-hydrogenated isoprene-styrene copolymer (SEPS), 35 parts by weight of naphthenic mineral oil, and 25 parts by weight of hydrogenated rosin.
[0035] The method for carrying out local electroplating protection with the elastic peelable adhesive in this embodiment is as follows:
[0036] (1) Put the elastic peelable glue into a temperature-controllable container, then heat it, and keep the temperature at 140-180°C. After the elastic peelable glue is completely melted, let it stand for 10-20 minutes to start using;
[0037] (2) The surface of the workpiece to be electroplated is first degreased and deoxidized, then rinsed and dried with clean water, and finally immersed in the melted elastic peelable glue, and taken out when the surface of the workpiece is completely immersed;
[0038] (3) Immerse the workpiece after dipping completely in cold water to cool for 10 minutes;
...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com