Coal mine underground coal bed waterproof paint
A waterproof coating and coal mine technology, applied in the field of waterproof coatings, can solve the problems of poor antistatic performance, large amount of polymer, poor flame retardancy, etc., to reduce unit water consumption, good impermeability, and sulfate resistance Good corrosion resistance and water resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] Add 14kg of redispersible latex powder, 35kg of slag cement, 35kg of quartz sand, 6kg of graphite powder, 10kg of fly ash, 4 of vermiculite powder, 6 of expanded perlite powder, 6kg of aluminum hydroxide, and 2kg of magnesium hydroxide. Mix evenly in the machine to get the powder; at the construction site, pour 55kg of mixing water into the mixer, then add 0.009kg of rosin air-entraining agent and 0.07kg of MELFLUX 1641F water reducer to the water and stir evenly, and mix the powder Pour into the agitator and stir at 300r / min for about 10min. After stirring evenly, you can start spraying. Test results: surface dry time, 1h; dry time, 8h; untreated tensile strength, 2.0MPa; untreated elongation at break, 40%; impermeable, 0.3MPa, 30min; flame retardancy and antistatic properties in line with coal Safety standard (MT113-1995), other performance indicators are qualified.
Embodiment 2
[0022] Add 20kg of redispersible latex powder, 40kg of silicate white cement, 40kg of quartz sand, 7kg of graphite powder, 10kg of fly ash, 5kg of vermiculite powder, 5kg of expanded perlite powder, 6kg of aluminum hydroxide, and 3kg of magnesium hydroxide. Mix evenly in the powder mixer to get the powder; at the construction site, pour 52kg of mixing water into the mixer, then add 0.09kg of rosin air-entraining agent and 0.08kg of MELFLUX 1641F water reducer into the water and stir evenly. Then pour the powder into the mixer, and stir at 300r / min for about 10 minutes, and spraying can be carried out after stirring evenly. Test results: surface dry time, 2h; dry time, 8h; untreated tensile strength, 1.9MPa; untreated elongation at break, 43%; impermeable, 0.3MPa, 30min; flame retardancy and antistatic properties in line with coal Safety standard (MT113-1995), other performance indicators are qualified.
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com