[0028] The light guide plate ink is prepared according to the composition ratio (mass percentage):
[0029] Urethane Acrylate 15%,
[0030] Polyester acrylate 50%,
[0031] Mix reactive diluent 15%,
[0032] Light reflective functional filler 15%,
[0033] Liquid paraffin 0.5%,
[0034] Dispersant 0.5%,
[0035] Photoinitiator (1173) 4.0%.
[0036] The preparation method comprises adding the above-mentioned components into a stirring device according to the formula ratio, and then grinding on a grinder until the particle size is 1-5 μm, and then packing.
[0037] Effect: The ink has excellent brilliance, the adhesion to acrylic is grade 1, the ink has good separation and release, and the curing time is 15 seconds.
Embodiment 2
[0039] The light guide plate ink is prepared according to the composition ratio (mass percentage):
[0040] Urethane Acrylate 20%,
[0041] Polyester Acrylate 40%,
[0042] Mix reactive diluent 10%,
[0043] Light reflective functional filler 26%,
[0044] Liquid Paraffin 1.0%,
[0045] Dispersant 0.5%,
[0046] Photoinitiator (1173) 2.5%.
[0047] The preparation method includes adding the above-mentioned components into the stirring device according to the formula ratio, and then grinding on the grinder until the particle size is 1-5 μm, stopping the grinding and packaging.
[0048] Effect: The ink has excellent brilliance, the adhesion to acrylic is grade 1, and it is easy to dry (good ink separation and release). The drying time is 15 seconds.
Embodiment 3
[0050] The light guide plate ink is prepared according to the composition ratio (mass percentage):
[0051] Urethane Acrylate 25%,
[0052] Polyester Acrylate 35%,
[0053] Mix reactive diluent 15%,
[0054] Light reflective functional filler 20%,
[0055] Liquid paraffin 1%,
[0056] Dispersant 1%,
[0057] Photoinitiator (1173) 3%.
[0058] The preparation method includes adding the above-mentioned components into the stirring device according to the formula ratio, and then grinding on the grinder until the particle size is 1-5 μm, stopping the grinding and packaging.
[0059] Effect: The ink has excellent brilliance, the adhesion to acrylic is grade 1, and it is easy to dry (good ink separation and release). The drying time is 15 seconds.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com