Method for preparing environment-friendly type casting adhesive agent
A binder and environment-friendly technology, applied in casting molding equipment, casting molds, cores, etc., can solve the problems of complex synthesis process, high casting cost, environmental pollution, etc., achieve simple production process, reduce casting cost, heat The effect of low decomposition temperature
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0018] The preparation process of casting binder of the present invention:
[0019] (1) Add animal glue and water to the reaction kettle, soak at room temperature for 30 minutes, heat and dissolve the animal glue after swelling to obtain animal glue liquid.
[0020] (2) In the prepared animal glue (1), add the fatty acid, alcohol and catalyst in the formulated amount, and react at 80-100° C. for 60-90 minutes. Then, when the temperature is lowered to 40° C., an anticoagulant in a formulated amount is added, and the reaction is continued for 30 minutes, and then the material is discharged to obtain the casting binder of the present invention.
[0021] Mold preparation process: add quartz sand, environment-friendly casting binder, and hardening accelerator into the sand mixer according to the formula, mix evenly, pour into the mold for compaction, and blow carbon dioxide to make the mold type hardening. It is characterized in that the weight percentage of each component in the...
Embodiment 1
[0026] An environment-friendly foundry binder, which is composed of animal glue, sebacic acid, ethanol, concentrated sulfuric acid, anticoagulant and water, and the weight percentage of each component content is:
[0027] Glue 30 Sebacic acid 20
[0028] Alcohol 10 Anticoagulant 10
[0029] concentrated sulfuric acid 1 water balance.
[0030] First add animal glue and water into the reaction kettle, soak at room temperature for 30 minutes, heat and dissolve the animal glue after swelling to obtain animal glue glue. Then add sebacic acid, ethanol and concentrated sulfuric acid according to the formula, and react at 80-100°C for 60-90 minutes. Then, when the temperature is lowered to 40°C, the anticoagulant in the prescribed amount is added, and the reaction is continued for 30 minutes before discharge to obtain an environment-friendly casting binder.
[0031] The preparation method of the casting mold: add 80g of quartz sand, 10g of environmentally friendly casting binder an...
Embodiment 2
[0033] An environment-friendly foundry binder, which is made of animal glue, oleic acid C 18 , ethanol, concentrated sulfuric acid, anticoagulant and water, etc., the weight percentage of each component content is:
[0034] Glue 45 Oleic C 18 20
[0035] Alcohol 10 Anticoagulant 15
[0036] concentrated sulfuric acid 1.5 water balance.
[0037] First add animal glue and water into the reaction kettle, soak at room temperature for 30 minutes, heat and dissolve the animal glue after swelling to obtain animal glue glue. Then add oleic acid, ethanol and concentrated sulfuric acid according to the formula, and react at 80-100°C for 60-90 minutes. Then, when the temperature is lowered to 40°C, the anticoagulant in the prescribed amount is added, and the reaction is continued for 30 minutes before discharge to obtain an environment-friendly casting binder.
[0038] The preparation process of the mold is carried out by the same mold preparation process as in Example 1.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com