Resist calcification modified method of heterogeneity biological organization material
A biological tissue and tissue material technology, applied in medical science, prosthesis, etc., can solve the problems of calcium salt deposition, no cross-linking, easy tearing, etc., achieve high tensile strength and elongation at break, biomechanical Enhanced performance, enhanced biostability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0087] Example 1 Using tannic acid alone to cross-link the bovine jugular vein with valve;
[0088] (1) Reagent preparation
[0089] 2.5% pH4.0 tannic acid solution: get 12.5 grams of commercially available tannic acid and dissolve it in 50mmol / LNa2HPO4 solution to 500ml, adjust the pH to 4.0 with hydrochloric acid.
[0090] (2) Material preparation
[0091] The bovine jugular vein pipeline with a diameter of 12-24 mm was collected and the length was about 10 cm. The fat and excess loose connective tissue on the surface were trimmed, and rinsed in D-Hank’s solution for later use.
[0092] (3) Cross-linking treatment process
[0093] 1. Rinse the inside and outside of the bovine jugular vein lumen with 2.5% pH4.0 tannin solution first, then fill the cavity with 2.5% pH4.0 tannin solution, and then insert 300ml of 2.5% pH4.0 Soak in a container of tannin solution for 48 hours at 32 °C.
[0094] 2. Before use, put the above-mentioned material treated by this method into norma...
Embodiment 2
[0114] Example 2 Synergistic crosslinking of tannic acid and glutaraldehyde to treat bovine jugular vein valved pipeline;
[0115] (1) Reagent preparation
[0116] 0.3% glutaraldehyde / 0.3% tannin mixed solution pH5.5: Dissolve 3ml of commercially available 50% glutaraldehyde solution in 50mmol / L Na 2 HPO 4 solution to 500ml, then take 0.5 g of commercially available tannic acid and dissolve it in the above solution, and adjust the pH to 5.5 with hydrochloric acid.
[0117] (2) Material preparation
[0118] Bovine jugular veins with a diameter of 12-24 mm and a length of about 10 cm were collected, the fat on the surface and excess loose connective tissue were trimmed, and rinsed in D-Hank’s solution for later use.
[0119] (3) Cross-linking treatment process
[0120] 1. Rinse the inside and outside of the cavity with 0.3% glutaraldehyde / 0.3% tannin mixed solution at pH5.5, then fill the cavity with 0.3% glutaraldehyde / 0.3% tannin mixed solution and put in 300ml Soak in a ...
Embodiment 3
[0141] Embodiment 3 Using tannic acid alone to cross-link the bovine pericardium;
[0142] (1) Reagent preparation
[0143] 1% pH5.5 tannic acid solution: prepare 50mmol / L Na 2 HPO 4 buffer solution to 500ml, then take 5 grams of commercially available tannic acid and dissolve it in the above solution, and adjust the pH value to 5.5 with hydrochloric acid.
[0144] (2) Material preparation
[0145] The collection area is about 8×8cm 2 Trim the fat and excess loose connective tissue from the bovine pericardium, rinse in D-Hank’s solution and set aside.
[0146] (3) Cross-linking treatment process
[0147] 1. Rinse the bovine pericardium material once with 1% pH5.5 tannic acid solution, then put it into a container containing 300ml of 1% pH5.5 tannic acid solution and fix it at 22°C for 96 hours.
[0148] 2. Before use, place the above-mentioned material treated by this method into normal saline and rinse it several times to remove residual tannin that has not been combine...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com