A production method and technology of bone china, applied in the field of ceramics, can solve the problems of transparency effect, lack of raw materials of bone ash, reducing mechanical strength, etc., so as to improve mechanical strength and thermal stability, improve porcelain quality and delicate feeling, and increase green strength. Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] Ingredients: ashes: 10%, kaolin: 30%, china stone: 52%, aluminum powder: 8% (percentage by weight). Batching, ball milling, sieving, dehydration, clay refining, molding, glazing, firing (firing temperature 1230 ° C ~ 1280 ° C, oxidizing flame firing) of the above raw materials can obtain good light transmittance, strength, heat stability. It is a new bone china with good properties, smooth glaze, and whiteness. After testing, the chemical composition of the body is: SiO2 54.5% Al2O3 26.3% P2O5 3.5% CaO 4.8% MgO 0.3% K2O+Na2O 3.6%. The amount of crystal phase accounts for 60% (weight percentage), the main crystal phase is mullite, and the secondary crystal phase is β-Ca 3 (PO 4 O) 2 , Anorthite, feldspar glass accounts for 31% (percentage by weight).
Embodiment 2
[0018] Ingredients: ashes: 6%, kaolin: 25%, porcelain stone: 60%, aluminum powder: 9% (percentage by weight). According to the process described in Example 1, the firing temperature is 1240°C to 1300°C. After testing, the chemical composition of the green body is: SiO2 56.2Al2O3 28.5% P2O5 2.1% CaO 2.9% MgO 0.2% K2O+Na2O 4.2% 5.9% loss on ignition, the amount of crystal phase in the porcelain body accounts for 65% (weight percent), the main crystal phase Mullite, the secondary crystal phase is β-Ca 3 (PO 4 O) 2 , Anorthite, and feldspar glass account for 32% (percentage by weight).
Embodiment 3
[0020] Ingredients: ashes: 8%, kaolin: 28%, china stone: 55%, aluminum powder: 9% (percentage by weight). According to the process described in Example 1, the firing temperature is 1240°C to 1300°C. After testing, the chemical composition of the green body is: SiO2 5.3% Al2O3 27% P2O5 2.8% CaO 3.9% MgO 0.4% K2O+Na2O 3.9% Burnout 6.7%. The amount of crystal phase in the porcelain body accounts for 64% (weight percentage), the main crystal phase is mullite, and the secondary crystal phase is β-Ca 3 (PO 4 O) 2 , Anorthite, and feldspar glass account for 34% (percentage by weight).
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com