preparation example Construction
[0037] A preparation method of viscoelastic polymer emulsion, comprising the following steps:
[0038] Step 1. In the jacketed reactor, add 30 to 47 parts of 3# white oil and 0.3 to 1 part of emulsifier in parts by mass, and start stirring to obtain the oil phase;
[0039] The emulsifier is Sorbitan oleate Span80, Sorbitan trioleate Span85, polyoxyethylene sorbitan monooleate Tween80, polyethylene glycol (400) dioleate polyDOPEG400 At least one of the emulsifiers is added in an amount of 10-20% of the total mass of the emulsion.
[0040] Step 2. In parts by mass, add 27 to 30 parts of the aqueous phase reaction monomer into the jacketed reactor, use 0.3 to 0.4 parts of 30% sodium hydroxide solution to adjust the pH to 5.5-6.8, and control the temperature to ≤20°C. Add 0.025 to 0.05 parts of oxidizing initiator and 0.04 to 0.06 part of co-initiator to obtain an aqueous phase;
[0041] The water-phase reaction monomer is a mixture of acrylamide, acrylic acid, 2-acrylamide-2-me...
Embodiment 1
[0053] A preparation method of viscoelastic polymer emulsion, comprising the following steps:
[0054] Step 1. In the jacketed reactor, add 30 parts of 3# white oil and 0.3 parts of sorbitan oleate Span80 in parts by mass, and start stirring to obtain the oil phase;
[0055] Step 2. In parts by mass, add 27 to 30 parts of water-phase reaction monomers into the jacketed reactor, use 0.3 parts of 30% sodium hydroxide solution to adjust the pH to 5.5-6.8, control the temperature to ≤20°C, and add 0.025 Part of potassium sulfate and 0.04 part of azobisisobutyl cyanide to obtain an aqueous phase;
[0056] The aqueous phase reaction monomer is a mixture of acrylamide, acrylic acid, 2-acrylamide-2-methylpropanesulfonic acid, N-allyl and N-alkyl amino acids, and the mass ratio is 100:10:10: 5.
[0057] Step 3. Press 52 parts of the water phase and 30 parts of the oil phase into the reaction kettle by mass parts, start stirring and emulsify with nitrogen for 30 minutes, and the tempe...
Embodiment 2
[0062] A preparation method of viscoelastic polymer emulsion, comprising the following steps:
[0063] Step 1. In the jacketed reactor, add 40 parts of 3# white oil and 0.6 part of sorbitan trioleate Span85 in parts by mass, and start stirring to obtain the oil phase;
[0064] Step 2. In parts by mass, add 28 parts of water-phase reaction monomers into the jacketed reactor, use 0.35 parts of 30% sodium hydroxide solution to adjust the pH to 5.5-6.8, control the temperature to ≤20°C, and add 0.35 parts of sulfuric acid Potassium and 0.5 part of azobisisobutyl cyanide to obtain an aqueous phase;
[0065] Described aqueous phase reaction monomer is the mixture of acrylamide, acrylic acid, 2-acrylamide-2-methylpropanesulfonic acid, N-allyl and N-alkyl amino acid, and the mass ratio is 100:25:15: 8.
[0066] Step 3. Press 60 parts of the water phase and 40 parts of the oil phase into the reaction kettle by mass parts, start stirring and nitrogen emulsification for 30 minutes, and...
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
shear viscosity | aaaaa | aaaaa |
viscosity | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com